ALTON
ENERuJI ‘QW-201 Section IX, ASME Boil
Procedure Qualification Record (PQR) [POR Nr:
ANK_14_B_02
ler and Pressure Vessel Code
Page: 1 of 2
Date 06/1212013
Ext Pon was quattes ae approve ome: Guan 4022 anv wast
wes no f
LEWES
ie L = J
wang Proceso: 200 t
ASMAWC sma
ype Manul/ Autom Som Auto. Deposited weld thickness SMAW.C:3mm, SMAW-B:7mm
Manual ‘Manual
acting Cv no
Base Metals (QW-403) fauines Clee! No
fasamtseees Apr aL [Arist Postweld Heat Treatment (aw-407)
free or cae: renperste
8 le NA
pmo: Pt topne: Pt Na
neeaese ot 2090" oa ing ae:
Dumetrot<24800: ote en
eon $m Gas (QW-408)
ewer: or “vinnn)
rei NA Shining:
Filler Metals (QW-404) rata
a a
2.5m. 25mm 12,5
Electrical Characteristics (aw-409)
Fier Wet Fo cna
as a pepe 200
oe . coum
AWS Caesteaton: ee “
esata _a&70v8_ fig 142.48 100-110 260-75
ow 18-18 2022 1!
Position (QW-405)
ey 0. Technique (QW-410)
CmainySounb
Wo Progression (Up, Downy sa
‘Down Usha fen
sung or Weave Beas
te: Sten
—_— sean:
Preheat (QW-406) Saniaeme
Prenat ton. SMAW:C SOmm/min SMAW-:35mnv/min
pone (pest:
Inarpase Temp
Max 200 6 siege or Mute Eeevoder:
ote: “Single
canna yes/no
Wenrsificati PQR Nr.
ALTON Procedure Qualification Record (PQR) JANK_14 B02
ENERJI QW-201 Section IX, ASME Boiler and Pressure Vessel Code |p, 2 of 2
Date 061272013
Tensile Test (QW150) (Report No: ER13-153-CEKME-07)
‘Specimen No. Dia. or Width Thicknes Area Ultimate Ultimate Type of Failure
Total Load | UnitStress | & Location
aw 462.1
mm mm mm kN Nimm?
SAMPLE 1 ‘8 927 im 208 590 Materia
SAMPLE? ‘8 927 17 18 an ator
Guided Bend Tests (QW160) (Report No: ER13-153-EGME-07)
Type FigureWo; QW4827 QWa823 it owes
SAMPLES ROOT BEND SATISFACTORY
SAMPLE-2 ROOT BEND SATISFACTORY
SAMPLES FACE BEND SATISFACTORY
SAMPLE-4 FACE BEND SATISFACTORY
Toughness Test (QW170) (N/A)
‘Specimen | Notch] — Notch Test —] apa Tater EX: Drop WarghT
No. | Location | ‘Type | Temperature | Values
ear] Ws Break | Wo Break
Fillet Weld Test (QW-180)(N/A)
Result -Satistactoy: Penetration nto Parent Metal
OYes LNo Dyes [INo
ype and Charecor of allure Macro - Rests:
other Tests
Type of Testis: RT report no ER-169-R7-10, esl satistcto, VT test report no N"VT:-ALTON.AMETTIN.002 result satisfactory
Deposit Analysis: si Mn e s cr Ni Mo
others:
HOSEYIN KENGERALAN
Welders Wave Groek Wo Samp Wo.
Az ALTUNTEPE BVT 261
ena; en13.453 oonanots AL inf
Laboratory Test No. Date ‘Signaty ’
We cert hatte statarnts inthe eco are coc anc that hotest welds fb ested in aZecranco wi he
reuoments of Seton Oo atest ston 0
wens 2 ony Bou Voe 0172008Procedure Qualification Record (PQR) |POR N":
ALTON ANK_14_B 01
ENERI QW-201 Section IX, ASME Boller and Pressure Vessel Code i
Page: 1 of
Date 06122013
Date PAR was quate and approved ois: onao2s 4022 anet0o
Ws No,
wrest a
ron CB BAe
A GTAW. 2 SMAW-B et
Deposited weld metal thickness: GTAW: 3mm, SMAW-B:@mm
if
sypoe Manus! Automatic Semi Autos
‘Manual Manual
2 sacking Chen no
Base Metals (QW-403) fetavere Cen No
Imeteraisees: asta Th Postweld Heat Treatment (aw-407)
hype or cede
108 aso.
pmo: Pt Pn: Pt
enna ot 50760) 40,9 7mm osino ra
Demeter st<020% 466 sn
mm A Samm Gas (aW-406) sows i
eter: oo Vinny
xin) sting
Ac 699.99 Ar 10-12
Filler Metals (QW-404) rat:
Wed Met Anata A No: =
ri at 3
1 122.500
Electrical Characteristics (aW-409)
a8 a ann 0c
penton: a
ae
ans caeteaton ne
senmasa 7018 (rn asots0 180-200 eens _
Masso 2202
Position (QW-405) _
reitoatccoe eo Technique (QW-410)
| Weld Progression (Uphill, Downhill): ‘ca
ope
ing orn Bed:
exter: Sra.
oxen
i
Preheat (QW-406) rave apnt
pasetteny GTS Stamin SMAW: 45min
romps Tmo
i
wens We Cony wee Vrs 02008if i i PQR Nr.:
ston |Procedure Qualification Record (PQR)|ink ‘4.5.01
ENERJI QW-201 Section IX, ASME Boiler and Pressure Vessel Code | nss5 2 of 2
ae 8/2013
Tensile Test (QW150) (Report No: ER13-153-GEKME-06)
Specimen No. | Dia.orwicth | Thickness area Ultimate timate | Type of Failure
Totaltoad | Unit stress | '& Location
aw 4524
mm mm mm? KN Nim?
SAMPLE 1 1 2 28 105,023 4s Weld nett
samPLe2 19 2 m0 109212 7a weld meta
Guided Bend Tests (QW160) (Report No: ER13-153-EGME-06)
Type FigureNo: —QWa822 GWa823 Resa WTS
SAMPLE ROOT BEND SATISFACTORY
SAMPLE ROOT BEND SATISFACTORY
SAMPLES FACE BEND SATISFACTORY
SAMPLE FACE BEND SATISFACTORY
Toughness Test (QW170) (N/A)
Specimen [Noten] Noteh Tost Tera Ep. Drop Weight
Wor” | vocation | "ype! | Tempore
Shox] Break] Wo Break
Fillet Weld Test (QW-180) (N/A)
Result Sattacto Penetration into Parent Meta:
Tyee Lino Dives Gino
Type and charactor of Faure Macro Results:
Other Test
Type of Teta): RT repr no ER-159-R7-07, esl saiacory VT test repo neNVTALTON-AMETINDY rau setstatoy
Deposit naysis: si Mn . s cr Ni Mo
ote
ALI BAKIR-
Weer Namo oak We Sampo,
i xa2im ALTUNTERE BVT 26
ERMA; ER13-153, 06/12/2013 Alte
Laboratory Test No. Date ‘Signafure ”
We caty hat he tater inthis recor ar cast and hath ost wads and tote in decordance with he
requremantsoitest edion of Sacton I ofthe ASME Cade
wens 2 Cony Bureau Vonas 012008