Professional Documents
Culture Documents
Jce 69 2017 7 5 1707
Jce 69 2017 7 5 1707
Autori:
Pregledni rad
Hussam K. Risan, Ibrahim S. I. Harba, Abdulkhalik J. Abdulridha
Numerika analiza ab zida s otvorom ojaanim CFRP-om podvrgnutim
ekscentrinim optereenjima
Subject review
Hussam K. Risan, Ibrahim S. I. Harba, Abdulkhalik J. Abdulridha
Numerical analysis of RC wall with opening strengthened by CFRP subjected
to eccentric loads
Dr.sc. Ibrahim S. I. Harba, dipl.ing.gra. Numerical analysis of the central hole in RC walls with and without CFRP, subjected
Sveuilite AL-Nahrain to uniform eccentric vertical line load, is presented in this paper. Six half-scale wall
Tehniki fakultet panels were modelled using the ABAQUS software to estimate the strengthening
Odjel za graevinarstvo effects. The analysis revealed that the load capacity of the wall in terms of maximum
Bagdad, Irak load carrying capacity is influenced by CFRP thickness. It was found that the
ibraharba@yahoo.com variation of CFRP thickness greatly influences the ultimate load carrying capacity,
crack patterns, principal plastic strain of concrete, and equivalent stress.
Key words:
RC wall with opening, CFRP, plastic damage (cracking) model for concrete
bersichtsarbeit
Hussam K. Risan, Ibrahim S. I. Harba, Abdulkhalik J. Abdulridha
Nummerische Analyse einer Stahlbetonwand mit einer CFRP-verstrkten
Dr.sc. Abdulkhalik J. Abdulridha, dipl.ing.gra. ffnung, die exzentrischen Belastungen ausgesetzt wird
Sveuilite AL-Nahrain
Tehniki fakultet In der Abhandlung wurde eine nummerische Untersuchung der mittleren ffnung in
Odjel za graevinarstvo Stahlbetonwnden mit und ohne CFRP-Verstrkung durchgefhrt, die einer exzentrischen
Bagdad, Irak vertikalen Belastung mit linearer Verstrkung unterzogen wurden. Sechs Wandplatten in einem
abdulkalikjabbar@yahoo.com Mastab 1 : 2 wurden im Computerprogramm ABAQUS zum Zwecke der Einschtzung der
Verstrkungswirkung modelliert. Die Analyse zeigte, dass die Tragfhigkeit der Wand im Sinne
der maximalen Belastung die Strke des CFRP beeinflusst. Festgestellt wurde, dass die Variation
der Strke des CFRP wesentlichen Einfluss auf die endgltige Tragfhigkeit, das Auftreten von
Rissen, die plastische Hauptverformung des Betons und die Vergleichsspannung hat.
Schlsselwrter:
Stahlbetonwand mit ffnung, CFRP, Modell der plastischen Abspannung (Rissbildung) des Betons
3. W3-T1, nosivi u jednom smjeru pridrani s dvije strane sa Tablica 2. Dimenzije primijenjenih CFRP traka [1]
CFRP trakama du strana otvora
4. W4-T0, nosivi u dva smjera pridrani s tri strane bez CFRP-a Duljina otvora irina otvora irina CFRP-a Duljina CFRP-a
[mm] [mm] [mm] [mm]
5. W5-T1, nosivi u dva smjera pridrani s tri strane sa CFRP
trakama dijagonalno prema otvoru
450 450 105 770 i 450
6. W6-T1, nosivi u dva smjera pridrani s tri strane sa CFRP-om
du strana otvora.
3. Metode i materijali
Svi zidovi bili su ispitani do sloma pod jednolikim uzdunim
optereenjem s ekscentrinou (tw/6). Zabiljeene su slike U ovom istraivanju nelinearna raunalna analiza provedena
pukotina i nosivost. Omjer pojaanja bio je isti u svim uzorcima je pomou raunalnog programa ABAQUS s konanim
zidova (promjer 4 mm, razmak od 100 mm i fy = 450 MPa) u elementima. Za modeliranje zida od armiranog betona
oba smjera i smjeten centralno u presjeku zida. Takoer, omjer koriteni su C3D4R (tetraedar s etiri vora i volumni
pojaanja odgovara minimalnim standardnim zahtjevima. elementi koji u svakom voru imaju tri translacijska stupnja
Svojstva CFRP-a i dimenzije navedeni su u tablicama 1. i 2., a slobode. U betonskim elementima, postoje dvije metode
slike 1. i 2. prikazuju uzorke zidova i konfiguraciju CFRP-a. za modeliranje pojaanja ipkama u ABAQUS-u. Armatura
se moe modelirati kao sloj unutar betonskog presjeka ili
Tablica 1. Svojstva CFRP-a: Sika Wrap-230C [1] diskretno kao tapni element koji je ugraen u beton. U
ovom istraivanju armatura je modelirana u obliku tapnih
Povrinska Modul Vlana Istezanje
teina
Debljina Gustoa
elastinosti vrstoa pri lomu
elemenata (konanih elemenata obostrano zglobnog tapa)
[mm] [g/cm3
] (T3D2) ugraenih u betonske prostorne elemente [16]. CFRP
[g/m2] [N/mm2] [N/mm2] [%]
traka predstavljena je s 4-vornim elementima ljuske. Treba
230 0,128 1,8 234000 4300 1,8 napomenuti da su u ABAQUS-u koriteni Odabrani parametri
Slika 1. AB zidovi nosivi u jednom smjeru (s dva pridranja) i konfiguracija CFRP-a [1]
Slika 2. AB zidovi nosivi u dva smjera (s tri pridranja) i konfiguracija CFRP-a [1]
modela za provoenje analize (kut dilatacije, = 33, vrno Hognestadovoj jednadbi [20, 21]. Pretpostavlja se veza bez
tlana deformacija c = 0,0002, neelastina deformacija proklizavanja (kruta veza) izmeu betona i CFRP-a [22].
betona u tlaku cin = 0,00082 do 0,0033, deformacija
betona pri pojavi pukotine u vlaku tck= 0,0002, a ostali 4. Rezultati i rasprava
podaci potrebni za model betona s mogunosti oteenja
(degradacije krutosti) u plastinom podruju, u ABAQUS-u Provjerit e se valjanost i uinkovitost numerikih rezultata
koriteni su sa zadanim vrijednostima). Rubni uvjeti zida za predloene modele materijala (betona, elika i CFRP-a)
na dnu su simulirani kao ekscentrini zglobni leajevi koji usporedbom s eksperimentalnim rezultatima. tovie,
omoguuju rotaciju, a na vrhu su klizni leajevi koji omoguuju provjere e se provesti usporeivanjem slike pukotina,
vertikalni pomak i rotaciju. Nadalje, na vrhu zida primijenjeno plastine deformacije betona i nosivosti dobivenih numeriki s
je jednoliko ekscentrino vertikalno optereenje kako bi se eksperimentalnim rezultatima od Lima i sur. [1].
simuliralo optereenje iz eksperimenta. Slika 3. prikazuje Tablica 3. prikazuje nosivost dobivenu eksperimentalnom i
model konanih elemenata, optereenja i rubne uvjete. numerikom analizom. Primjeuje se da su prosjena nosivost
elik se definira kao elastian-idealno plastian materijal kod numerike analize poveana za 0,533 % u usporedbi s
dok je CFRP definiran kao linearno elastian materijal. eksperimentalnim krajnjim optereenjem (num. optereenje
Beton je modeliran pomou modela plastinoga poputanja / eksp. optereenje) za zidove nosive u jednom smjeru, dok je
(raspucavanja) betona (eng. concrete damaged plasticity model nosivost dobivena numerikim proraunom smanjena za 2,8 % u
CDP model). Ovaj model su razvili Lubliner i sur. [17] i dalje usporedbi s eksperimentalnim krajnjim optereenjem za zidove
su ga nadograivali Lee i Fenves [18]. U ovom modelu prirast nosive u dva smjera.
naprezanja po plohi teenja se kontrolira sa svojstvima Slike 4. i 5. prikazuju eksperimentalne i numerike slike
betona u plastinom podruju za vlano i tlano naprezanje, pukotina i plastine deformacije betona u zidovima nosivim
[19]. Radni dijagram betona u tlaku u ovom radu temelji se na u jednom, odnosno dva smjera. Na slici 4, zabiljeene slike
Eksperimentalna Numerika
Debljina CFRP-a
Oznaka zida Konfiguracija CFRP-a Tip pridranja zida analiza analiza
[mm]
[kN] [kN]
W1-T0 - - s dvije strane 273,9 278,2
W2-T1 Nagnuto 45 0,128 s dvije strane 315,2 314,9
W3-T1 Oko 90 0,128 s dvije strane 348,5 349,3
W4-T0 - - s tri strane 450,0 448,2
W5-T1 Nagnuto 45 0,128 s tri strane 699,0 682,7
W6-T1 Oko 90 0,128 s tri strane 660,6 661,2
Slika 6.
Maksimalne plastine deformacije zida nosivog u jednom
smjeru i razliitim debljinama CFRP-a s nagibom prema otvoru
Slika 4.
Eksperimentalne i numerike slike pukotina i plastine Slika 7.
Maksimalne plastine deformacije zida nosivog u jednom
deformacije betona kod zidova nosivih u jednom smjeru smjeru i razliitim debljinama CFRP-a koji okruuje otvor
paralelno s njegovim stranama
Oznaka zida Konfiguracija CFRP-a Debljina CFRP-a [mm] Tip pridranja zida Numerika analiza [kN]
W2-T1 Nagnuto pod 45 0,128 s 2 strane 314,9
W2-T2 Nagnuto pod 45 0,256 s 2 strane 316,7
W2-T3 Nagnuto pod 45 0,348 s 2 strane 335,6
W2-T4 Nagnuto pod 45 0,512 s 2 strane 314,3
W3-T1 Oko 90 0,128 s 2 strane 349,3
W3-T2 Oko 90 0,256 s 2 strane 424,4
W3-T3 Oko 90 0,348 s 2 strane 433,8
W3-T4 Oko 90 0,512 s 2 strane 400,9
W5-T1 Nagnuto pod 45 0,128 s 3 strane 682,7
W5-T2 Nagnuto pod 45 0,256 s 3 strane 831,1
W5-T3 Nagnuto pod 45 0,348 s 3 strane 832,7
W5-T4 Nagnuto pod 45 0,512 s 3 strane 722,8
W6-T1 Oko 90 0,128 s 3 strane 661,2
W6-T2 Oko 90 0,256 s 3 strane 746,9
W6-T3 Oko 90 0,348 s 3 strane 826,2
W6-T4 Oko 90 0,512 s 3 strane 748,6
Slika 8. Maksimalne plastine deformacije zida nosivog u dva smjera i Slika 10. Von-Misesova naprezanja za zid nosiv u jednom smjeru i
razliitim debljinama CFRP-a s nagibom prema otvoru razliitim debljinama CFRP-a s nagibom prema otvoru
Slika 9. Maksimalne plastine deformacije zida nosivog u dva smjera Slika 11. Von-Misesova naprezanja za zid nosiv u jednom smjeru i
i razliitim debljinamaCFRP-a koji okruuje otvor paralelno s razliitim debljinama CFRP-a koji okruuje otvor paralelno s
njegovim stranama njegovim stranama
Slika 12.
Von-Misesova naprezanja za zid nosiv u dva smjera i
razliitim debljinama CFRP-a s nagibom prema otvoru Slika 13.
Von-Misesova naprezanja za zid nosiv u dva smjera i
razliitim debljinama CFRP-a koji okruuje otvor paralelno s
njegovim stranama
5. Zakljuak
Izrada numerikog modela kalibriranog prema rezultatima predvianja ponaanja AB zidova s otvorima pojaanih
eksperimentalnih istraivanja Lime i sur. [1] te numerika CFRP-om.
analiza uinaka poveanja debljine CFRP-a na ponaanje AB -- Numeriki rezultati vode do zakljuka da varijacija debljine
zidova s otvorima nosivih u jednom i dva smjera u vidu oblika CFRP-a ima znaajan utjecaj na nosivost, poloaj pukotina,
sloma i poloaja pukotina, oblika pukotina i nosivosti, dva su glavne plastine deformacije betona i ekvivalentno
glavna cilja ovog rada. Na temelju provedene analize mogu se naprezanje u trakama CFRP-a. Kada se debljine CFRP-a
donijeti sljedei zakljuci: poveaju na 0,348 mm, krajnja optereenja se takoer
-- Usporedba numerikih rezultata na temelju modela poveavaju i raspodjela pukotina postaje povoljnija zbog
betona s mogunosti oteenja (degradacije krutosti) poveanja nosivosti na savijanje AB zidova. Uinak ovog
u plastinom podruju i eksperimentalnih rezultata, i u poveanja postaje stabilan oko kritine vrijednosti debljine
smislu nosivosti i oblika pukotina, pokazuje na sposobnost CFRP-a koja je priblino jednaka povrini glavne armature za
predloene analize konanim elementima vrlo dobrog pojaanje u zidu zbog otvora.
LITERATURA
[1] Lima, M.M., Doh, J.H., Miller, D.: Experimental Study of RC Walls [6] Enochsson, O., Lundgvist, J., Taljsten, B., Rusinowski, P., Olofsson,
with Opening Strengthened by CFRP, 23rd Australian Conference T.: CFRP strengthened openings in two-way concrete slabs: an
on the Mechanics of Structures and Materials (ACMSM23), ed. experimental and numerical study, Construction and Building
Smith, S.T., Byron Bay, Australia, 9 12 December 2014. Materials, 21 (2002) 4.
[2]
Sas, G.: FRP Shear Strengthening of RC Beams and Walls, [7]
ACI 318M-14, Building Code Requirements for Structural
Department of Civil, Mining and Environmental Engineering, Lulea Concrete, American Concrete Institute, Detroit, USA
University of Technology, Licentiate Thesis, 2008. [8]
AS3600-2009, Concrete Structures, Standards Australia,
[3] Bozdogan, K.B.: A method for free vibration analysis of stiffened Sydney, Australia, 2009. Casadei, P., Ibell, T., and Nanni, A.
multi-bay coupled shear walls, Asian Journal of Civil Engineering, (2003). Experimental results of one-way slabs with openings
7 (2006) 6. strengthened with CFRP laminates. Fibre-reinforced polymer
[4]
Elnashai, A., Sarno, L.: Fundamentals of Earthquake reinforcement for concrete structures FRPRCS6.
Engineering, John Wiley, New York, 2008, https://doi. [9]
Lombard, J.: Seismic Strengthening and Repair of Reinforced
org/10.1002/9780470024867 Concrete Shear Walls Using Externally Bonded Carbon Fibre Tow
[5] Bhinia, D., Prakash, V., Pandey, A.D.: A procedure for evaluation Sheets, Department of Civil and Environmental Engineering,
of coupling beam characteristics of coupled shear walls, Asian Carleton University, Master of Engineering thesis, 1999. (Cited in
Journal of Civil Engineering, 8 (2007) 3. Ref. 1)
[10] Sugiyama, T., Uemura, M., Fukuyama, H., Nakano, K., Matsuzaki, [16]
Kwak, H.G., Kim, D.Y.: Nonlinear analysis of RC shear walls
Y.: Experimental study on the performance of the RC frame in considering tension stiffening effect, Computers and Structures,
filled cast-in-place on-structural RC walls retrofitted by using 79 (2001).
carbon fibre sheets, Proceedings of the 12th World Conference on [17]
Lubliner, J., Oliver, J., Oller, S., Onate, E.: A plastic damage
Earthquake Engineering, New Zealand, Paper No. 2153, 2000. model for concrete, Int J Solids Struct, 25 (1989) 3, https://doi.
[11] Antoniades, K.K., Salonikios, T.N., Kappos, A.J.: Cyclic tests on org/10.1016/0020-7683(89)90050-4
seismically damaged reinforced concrete walls strengthened [18]
Lee, J., Fenves, G.L.:Plastic-damage model for cyclic loading
using fibre -reinforced polymer reinforcement, ACI Structural of concrete structures, J Eng Mech, 124 (1998) 8, https://doi.
Journal, 100 (2003) 4. org/10.1061/(ASCE)0733-9399(1998)124:8(892)
[12] Li, Z.J., Balendra, K.H., Tan, K.H.: Finite Element Modeling of Cyclic [19] Hibbitt, Karlsson & Sorensen Inc., ABAQUS theory manual, user
Behaviour of Shear Wall Structure Retrofitted Using GFRP, ACI-SP, manual and example manual, Version 6.8, Providence, RI, 2008.
2005.
[20] Hognestad, E.: A study on combined bending and axial load in
[13] Doh, J.H., Fragomeni, S., Loo, Y.C.: Evaluation of experimental reinforced concrete members, University of Illinois Engineering
behaviour of normal and high strength reinforced concrete walls Experiment Station, University of Illinois at Urbana-Champaign,
in two-way action, Proceedings of the 17th Advanced in Mechanics IL, (1951).
of Structures and Materials, Gold Coast, Australia, June, (2002).
[21]
Mostofi Nejad, D.: Reinforced Concrete Structures. Vol.1. 14th
[14]
Doh, J.H,. Fragomeni, S.: Evaluation of experimental work on edition, Esfahan: Arkane Danesh, 2009.
concrete walls in one and two-way action, Australian Journal of
[22]
ACI Committee 440.2R 2002., Guide for the Design and
Structural Engineering, 6 (2005) 1.
Construction of Externally Bonded FRP Systems for Strengthening
[15] Mohammed, B.S., Ean Malek, L.: One way RC wall panels with Concrete Structures.
openings Strengthened with CFRP, construction and building
materials .