PLAN DE GESTION DE CALIDAD SM/QCRWPS.01
ESPEGIFICAGION DEL PROCEDIMIENTO DE SOLDADURA [HOA det
ee _DICION 1
De acuerdo al oédigo AWS D1.1/01.1M:2018 MISION ene-16
WELDING PROCEDURE SPECIFICATION (WPS)
PREQUALIFIED ‘QUALIFIED BY TESTING
or PROCEDURE QUALIFICATION RECORDS (PQR)
dentication # — __su-wes.o2
ompany Name SMA METAL INDUSTRIAL Revision _1 Dato 00/276 By __Jamos Ru
elding Process(es) GMAW. ‘Authorized by lames Ruiz Date 0912/16
jpporting PAR N’ (3) Precaliicado Type Manual ‘Semi-Automatic 1X
Machine ‘Automatic
JOINT DESING USED
yee TCFI-GF [ J POsTION.
ingle Double Weld Position of Groove Fille
sacking: No Ex Vertical Progression Up Dow
Backing Mater =
001 Opening _0- 5mm _Root Face Dimension [HEECTRIGAT CHARACTERISTICS |
roove Angle Radius (-U) 7
leack Gouging Yes NoLx ‘Transfer Mode (GMAW) Shot-Ciruting
Method: = Globular Pulsed spray [Xx
BASE METALS J Curent: Ac ocer[X] _ ocen|
alorial Spec. ‘other
[Type or Grade “Tungsten Electrode (GTAW)
[Thickness: “Groove = Filet 30 nasta Size =
menor a 75 Type
WS Specification ‘AWS A518 TECHNIQUE
WS Classification “AWS ER 705 6 ‘Stinger or Weave Bead: Weave
Mut-pass or Single Pass (per si) Sige
Number of Electrodes ‘Only
Fux ‘Gas Electrode Spacing Longitudinal =
‘Composiion _60% Ar-20% CO, Lateral =
tectrode-Fix(class) _—~__FlowRete 15-25 i Angle
‘Gas Cup Siz 10-15 mm Contact Tube to Work Distance,
Peening ~
PREHEAT Interpass Cieaning ‘Grinding and Wire Brish
Pretest Temp. Min T.amb (20.0 25°C)
nterpass Temp. Min = Max Temp. —
Time =
Ss Wer bnig PRocepuRe:
Pass or Filler Metals Current 2
weld | Process Vous} Travel Speed
eae ciass | pam | yPe® | Ampsor Wire (cmvimin)
Polarity | Feed Speed |
1 | emaw [er 7056|iomm| ocep | 220+ 10% | 267% | 1602 26% 1]
J bm
TO-F12.6F
[Aerobade por Ing. James Ruiz A
oye
4
6} exe. 2017