DRYING CYCLE

Log firing 24 hours up to kiln o/L hood reaches 250c


250c /hr up to 1050c -> 3days
Oil flow rate 40litters /hr -100litters
Cooler main door open
Cooler oversize chute open
All slip seals full open
Emergency cap fully open
Combustion air 1000-1500 Nm3hr
Reg no QRT 6 and 7 avg
Kiln position no QRT 6 at 3 0, oclock position
Kiln ½ rotation for ever 8hours 1st day
6hours 2nd day
4hours 3rd day
Kiln inlet hood should raise 60-700c
Complete the drying cycle
Raise the temperature 30-400c/hr up to 500-6000c
Close over size chute
Cooler main door close slowly
Close from 3000c on wards
Dsc temperature 180-2500c
Two days
Raise the temperature 600-10000c at 500c/hr
Continuously rotation at 7000onwards
Start injection coal 0.5 t/h fines and medium
7th 6th 1000- 1050
5th 4th 1000-1050
3rd 2nd 1000-980
Feed start at first zone temperature reaches 6500c

S.N DESCRIPTION SPECIFICIATION QUNTITY

1 S.S.304 -8MM DIA TYPE V 85 3200


2 S.S.304 -8MM DIA TYPE V 125 8100 C
3 S.S.304 -8MM DIA TYPE V150 26600
4 S.S.304 -8MM DIA TYPE V 55 1200
5 S.S.304 -8MM DIA TYPE V 45 6000
6 S.S.304 -8MM DIA TYPE V 100 2500
7 S.S.304 -6X25MM FLATE TYPE FLAT Y - 100 1300
8 S.S.304 -6X25MM FLATE TYPE FLAT Y - 200 2400 KI
9 S.S.304 -5X25MM FLATE TYPE FLAT Y - 230 3150
FLAT 50 50 6 DIA 10 HOLE
10 CENTER TYPE FLAT Y - 175 26600