Professional Documents
Culture Documents
Original Article
Keywords: The correlation between the choice of reference material and model utilized in determining fracture toughness
Fracture toughness from indentation-induced radial cracks was critically investigated with six commonly used reference materials.
Radial crack Initially, the empirical constants in Anstis’s and Laugier’s equations were calculated, compared and analyzed.
Nanoindentation According to the values of the constants, the reference materials were categorized into three groups. This
Reference materials
classification was further verified by evaluating the corresponding constants of 13 additional equations. To
Diamond/SiC composite film
account for the classification, FIB technique was employed to examine the crack morphology in the reference
materials – Si (100) features an almost Half-penny-shaped crack while the cracks in SiC (0001) display nearly as
a rectangle, both far from the assumptions employed by the models. Subsequently, an improved and more
reliable procedure to determine fracture toughness is proposed. Finally, with this procedure, the fracture
toughness of a diamond/SiC composite film is determined to be 11.1 ± 1.1 MPa m1/2.
1. Introduction Fig. 1(a)). [4]. In 1987, Laugier [5,6] found that ceramics typically
display a Palmqvist type (Fig. 1(b)) instead of Half-penny type crack
The determination of fracture toughness from the length of in- morphology and modified Anstis’s equation by adding the term (l/a)−1/
2
dentation induced radial cracks is a widely used strategy, the origin of to Anstis’s equation (c/a ≥ 1.3), see Eq. 2 (l represents the crack
this concept dates back to 1957 when Palmqvist [1,2] proposed an length measured from the corner of the remaining imprint of the in-
empirical relation between crack length and the maximum applied denter to the end of the crack). He argued that Anstis’s equation is able
load. In 1980, Lawn, Evans and Marshall (LEM) proposed a fracture to reliably describe Palmqvist crack to some extent as the additional
toughness equation based on elastic-plastic fracture mechanics, Eq. 1 term often only features a minor impact on the relationship. Both An-
[3], where E, H, Pmax, c and χ are elastic modulus, hardness, maximum stis’s and Laugier’s equations allow us to estimate fracture toughness
indentation load applied, total crack length, and a dimensionless con- from directly measurable parameters (e.g. E, H, Pmax, c, l and a). In
stant, respectively. It should be noted here, that in order to render the addition to Anstis’s and Laugier’s equations, a diversity of equations
indentation-based fracture toughness discussed in this work compliant dealing with fracture toughness determination from radial crack length
with modern standards and nomenclature, KIF (indentation fracture have been proposed in the 1980s, which are based on Anstis’s equation.
toughness) will be used instead of KIC in all original fracture toughness However, these equations only exhibit slight changes to the exponent n
equations throughout this work. In 1981, Anstis employed a number of in the (E/H)n part and additional changes to the dimensionless con-
reference materials including mono-, polycrystalline and amorphous stant. A systematic work reviewing these equations has been carried out
ceramics, which covered a large regime of fracture toughness values by Ponton et al. [7], in which they summarized nineteen equations from
ranging from 0.74 to 12 MPa m1/2, and carried out corresponding tests different references into 7 generic equations.
with a Vickers indenter to derive the dimensionless constant in Eq. 1
KIF = χ (E/H)1/2 Pmax c−3/2 (1)
and ended up with a value of χ = 0.016 ± 0.004. Thereafter, this
equation is frequently referred to as Anstis’s equation. It is based on a KIF = χv (E/H)2/3 (l/a)−1/2 Pmax c−3/2 (2)
Half-penny crack type and the boundary condition that c≫a is sug-
gested (c is the total crack length, whereas, a denotes the crack length In recent years, the validity of fracture toughness determination
measured from the center to the corner of the remaining imprint, see from radial cracks has triggered intense debate. Quinn and Morell et al.
[8–10] argued that the fracture toughness equations have various
⁎
Corresponding authors.
E-mail addresses: thorsten.staedler@uni-siegen.de (T. Staedler), xin.jiang@uni-siegen.de (X. Jiang).
https://doi.org/10.1016/j.jeurceramsoc.2019.10.013
Received 27 June 2019; Received in revised form 2 October 2019; Accepted 4 October 2019
Y. Guo, et al.
Table 1
Summary of some important parameters utilized in references to derive empirical constants.
Year Researcher Indenter type Crack morphology Equation used Constant Reference material
1981 Anstis [4] Vickers Half-penny Eq. 1 0.016 ± 0.004 Si3N4, Al2O3, glass ceramic, glass
1987 Laugier [6] Vickers Palmqvist Eq. 2 0.015 Data from Anstis
1994 Harding [17] Cube-corner Radial cracks Eq. 1 0.036 Fused quartz, Ge (111), pyrex, Sapphire (111), Si (100), Si (111), SiC, Si3N4, Soda
lime glass, spinel (100)
2012 Cuadrado [16] Berkovich Palmqvist Eq. 1 0.026 ± 0.001 Si (100), SiC (0001), soda-lime glass
Eq. 2 0.022 ± 0.001
Cube-corner Palmqvist Eq. 2 0.057 ± 0.002
Y. Guo, et al.
Table 2
Hardness and elastic modulus of the six reference materials.
Material Elastic modulus* (GPa) Hardness (GPa) Poisson ratio
[21–23]
crystalline silicon with two orientations (Si (100) and Si (111)), soda-
lime glass, single crystalline silicon carbide (SiC (0001)), sapphire and
fused quartz were chosen as reference materials to study fracture
toughness and its correlation to the equations utilized for determina-
tion.
Prior to accessing fracture toughness, a Berkovich indenter with a
maximum load of ˜10 mN was employed to evaluate hardness and Fig. 2. A schematic diagram illustrating the procedure utilized to obtain in-
elastic modulus of the reference materials. The results of each material formation about the crack morphology: The reconstruction is realized by cri-
were derived from an average of more than 50 measurements and are tically analyzing a series of cross-sections along the indentation crack.
listed in Table 2. Loading and unloading rate were held constant for
each sample. The analysis of the load-displacement curves was based on shown in Fig. 3. The triangular imprints caused by the three-sided
the method proposed by Oliver and Pharr [17]. The initial contact was Berkovich indenter can be readily observed. Additionally, radial cracks
determined by assuming a tip rounding and fitting the first few nan- emanating from the corners of the indentation impressions can be
ometers (˜10 nm) of the load-displacement curves with a P = C·(h’-h0)3/ noted, while no signs of lateral cracks, delamination, chipping or
2
relationship. [18] In order to generate cracks, a high load Berkovich spalling is observed. In this context, fused quartz represents an excep-
indenter (10 N) was employed. In this context, it is worthwhile to tion as it exhibits frame-like cracks/cone cracks, which are presumably
mention, that all crack tests were carried out in a displacement con- caused by a different crack mechanism. This finding agrees well with
trolled manner rather than a load controlled one. This choice was made Cook et al.’s report. [20] They observed the appearance of cone cracks
due to the fact that fracture is often accompanied by a sudden change in in fused quartz at a very early stage in the loading cycle prior to the
displacement, thus load controlled manner potentially might add extra formation of radial cracks.
work to the system and consequently affect the crack length. For sta- Based on the mechanical properties of the reference materials along
tistical reasons, about 30 crack tests were performed at various max- with their corresponding crack dimensions (c, a and l), the empirical
imum load for each sample of interest. Subsequently, the crack lengths constants in Anstis’s and Laugier’s equations can be calculated. In
(c, l and a) were examined and measured using a scanning electron Anstis’s equation, KIF (H/E)1/2 c3/2 is plotted against P and the slope of
microscope (SEM, Zeiss Ultra 55). The actual position of the crack tips is this relationship is taken as the empirical constant χ. Likewise, in
determined at high magnification to ensure an accurate measurement Laugier’s equation, KIF (H/E)2/3 (l/a)1/2 c3/2 is plotted against P and the
of the crack length. Most importantly, to exclude the potential com- corresponding slope is taken as the empirical constant χv. The fracture
plexity of multiple cracks, only indentations solely featuring radial toughness values used in these equations stem from well-accepted
cracks (judging by the top-view SEM images) and not showing any R- conventional methods in literatures (values are given in Table 3)
curve behavior were used to calculate fracture toughness. All other ones [16,21–23]. The KIF (H/E)1/2 c3/2 – P and KIF (H/E)2/3 (l/a)1/2 c3/2 – P
that show lateral cracks, delamination, chipping or spalling at enhanced relationships mentioned above are displayed in Fig. 4.
indentation loads were discarded in this work. Overall, the data points of Si (100), Si (111), soda-lime glass, SiC
In order to investigate the details of crack morphology below the (0001) and sapphire exhibit an almost linear relationship with respect
materials surfaces, the focus ion beam (FIB, Helios NanoLab 600) cross- to both equations. However, the data points of fused quartz do not fall
sectioning was utilized to create a series of cross-section images along on this relationship. The reason for this, as mentioned before, pre-
the crack as shown in Fig. 2. Sequentially, the crack morphology can be sumably lies in fused quartz’s tendency to show cone cracks prior to
reconstructed from the crack lengths observed on the various cross- radial cracks, see Fig. 3. In Anstis’s research [4], a variety of materials
sections. In general, 5 or more cross-sections are created for the re- featuring a wide range of fracture toughness values were fitted together
construction depending on the total crack length. to obtain a global constant. Therefore, using the same strategy and
Finally, a diamond/SiC composite film deposited by microwave fitting the reference materials used here as a whole dataset (except for
plasma chemical vapor deposition (MPCVD) was investigated. The de- fused quartz), results in a global constant of ˜0.025. In comparison,
tails of the growth parameters as well as the strategy to access its Cook got a value of 0.022 for a variety of ceramics and glasses exposed
hardness and elastic modulus are given elsewhere. [19] Lastly, the to ambient air with a Vickers indenter [24,25] and Cuadrado obtained
fracture toughness of this diamond/SiC composite film was evaluated 0.026 ± 0.001 for Si (100), SiC (0001) and soda-lime glass with a
using the criterion developed within this work. Berkovich indenter [16]; both findings are in good agreement with our
results. Similarly, fitting with Laugier’s equation will give a global
3. Result and discussion constant of ˜0.022, which is identical to the one presented by Cua-
drado’s [16]. Consequently, the results we’ve obtained so far for the
3.1. The examination of Anstis’s and Laugier’s equations reference materials used here are in excellent agreement with existing
literatures.
Anstis’s and Laugier’s equations are the first that are examined with Nevertheless, a closer look at the lower load regime reveals that, the
respect to the six reference materials as they are likely the most widely linear relationships actually differ for the various reference materials.
used equations for fracture toughness determination based on radial The latter implies that their crack behavior is best described by dif-
cracks. The top-views of the indented surface region post testing are ferent empirical constants. The details of the KIF (H/E)1/2 c3/2 – P and
Y. Guo, et al.
Fig. 3. SEM images of the indent imprints on reference materials (a) Si (100), (b) Si (111), (c) soda-lime glass, (d) SiC (0001), (e) sapphire and (f) fused quartz.
Table 3
Calibration of the constants χ and χv in Anstis’s equation and Laugier’s equation for Berkovich indenter.
Material χ in Anstis’s equation KIF (H/E)1/2 c3/2 = χP χv in Laugier’s equation KIF (H/E)2/3 (l/a)1/2 c3/2 = χvP Fracture toughness used for equation fitting (GPa m1/
2
)
Fig. 5. (a) KIF (H/E)1/2 c3/2 – P relationship for the calculation of χ in Anstis’s
Fig. 4. A Berkovich indenter is employed to induce cracks in six reference equation; (b) KIF (H/E)2/3 (l/a)1/2 c3/2 – P relationship for the calculation of χv
materials at various maximum indentation load. (a) shows the KIF (H/E)1/2 c3/2 in Laugier’s equation at lower loads corresponding to Fig. 4 (a) and (b), re-
– P relationship for the calculation of χ in Anstis’s equation; (b) displays the spectively.
relationship of KIF (H/E)2/3 (l/a)1/2 c3/2 – P for the calculation of χv in Laugier’s
equation. Details of the data points at low load (highlighted in red) are pre-
sented in Fig. 5 and will be discussed in the text. (For interpretation of the is 0.025 and barely varies when changing to Laugier’s equation. The reason
references to colour in this figure legend, the reader is referred to the web behind this lies in the l to a ratio range and will be discussed in detail in
version of this article.) Section 3.2. The constant of SiC (0001) is calculated to be 0.037 in Anstis’s
equation and 0.024 in Laugier’s equation. Finally, sapphire shows similar
KIF (H/E)2/3 (l/a)1/2 c3/2 – P relationships at the lower load regime are numerical results to SiC (0001). Considering the non-ideal crack mor-
shown in Fig. 5. The large number of experimental data points allows phology in real measurements and the different loading regimes applied to
for a detailed insight into this phenomenon. At lower loading regime, initiate cracks for different reference materials, it is speculated that to some
the linear relationships for Si (100) and Si (111) clearly differ from that extend sapphire’s crack behavior resembles the one shown by SiC (0001)
of SiC (0001); the latter shows a significantly steeper slope, i.e. em- rather than that of Si or soda-lime glass.
pirical constant. In order to get an overview of the differences in con- At this point, we can summarize the findings presented so far as fol-
stants received for the various reference materials, the numerical results lows: In the first part of this section, the global empirical constants of
of the linear fitting of the individual materials are listed in Table 3. Anstis’s and Laugier’s equations have been calculated with a dataset
Of all calculated constants of the reference materials, the constants of consisting of all reference materials (except for fused quartz). In the second
fused quartz are significantly lower than the constants of the other mate- part, the individual constants are calculated for each reference material,
rials in both fitting scenarios, which is in accordance with the experimental respectively. Subsequently, now the relationship between the global and
results shown in Fig. 4. Hence, in later discussions, fused quartz will mostly the individual constants needs to be examined from a pure mathematical
be excluded. Moreover, it is noticeable that Si (100) and Si (111) behave point of view. Mathematically, the global linear fitting (of the first part)
almost identically in both scenarios. Although crystal anisotropy may result will try to match the data points of soda-lime glass in order to reduce the
in slight change in fracture toughness, it is confirmed that the discrepancy associated R square (R2) because of the large maximum load it requires to
is less significant when indenting (100) and (111) planes. [16,26] With crack the glass. Thus, in the case of a linear fitting with Anstis’s equation,
Anstis’s equation, a constant of 0.024 has been achieved for Si (100) and Si the data points of SiC (0001) and sapphire play a minor role since their
(111), which is very close to the one reported by Pharr, 0.0237, in the indentation load range sufficient for cracking is significantly smaller
context of a study dedicated to the effect of the indenter angle on the compared to the one necessary to crack the soda-lime glass. Consequently,
cracking of Si [27]. In the case of Laugier’s equation, Si (100) and Si (111) the global constant will always be close to the individual one of soda-lime
result in constants of ˜0.015. The constant of soda-lime glass in Anstis’s case glass, Si (100) and Si (111). Furthermore, the fracture toughness of these
materials agrees well with the corresponding information gained by
Y. Guo, et al.
conventional methods. Moreover, there is no doubt that the fracture indenting low fracture toughness materials with a Vickers indenter
toughness of SiC and sapphire will be underestimated when calculated generally leads to the formation of a Half-penny crack whereas high
using this global constant. In the case of a linear fitting with Laugier’s fracture toughness materials show Palmqvist cracks [28]. Following
equation, the global constant will be close to the individual one of soda- this argument, the crack morphology might be the reason for the
lime glass, SiC (0001) and sapphire. Thus, the fracture toughness of these classification of reference materials and will be discussed in Section 3.3.
three reference materials agrees well with conventional results while the Based on the discussions above, the six reference materials studied
fracture toughness of Si (100) and Si (111) will be overestimated. Findings here can be classified into three groups: Group I: Si (100), Si (111),
like these of an underestimated fracture toughness for SiC or sapphire or soda-lime glass; Group II: SiC (0001), sapphire; Group III: fused quartz.
an overestimated fracture toughness for Si are often reported in literature
[4,16]. Therefore, the discussion presented above is helpful in order to
3.2. The investigation of other equations
resolve some of the irritations caused by under- or overestimated fracture
toughness values obtained for some reference materials under certain
In this section, the equations summarized in Ponton’s work [7] have
boundary conditions. Furthermore, it became obvious that the reference
been reexamined with respect to their empirical constants in order to
materials most widely used for fracture toughness evaluation based on
further test the validity of the classification idea. In all considerations,
radial cracks actually show quite a diverse behaviors. Hence, a possible
the value of the constants is calculated for the six reference materials
solution to solve the issues mentioned above could be to classify the re-
using the same procedure and strategy as described in Section 3.1. It is
ference materials into groups. In that case, a group would be composed of
noteworthy that, once the equations are investigated from the per-
materials featuring similar constants in the corresponding fracture
spective of the empirical constant, a substitution of Hv (load/real con-
toughness equation. For example, Si (100) and Si (111) belong to one
tact area) by H (load/projected contact area) does not result in any
group while SiC (0001) and sapphire are part of another group.
differences for some of the equations.
The exponential relationship between the maximum load P and total
In Ponton’s work, 19 equations based on different physical models
crack length c for reference materials is depicted in Fig. 6. It can be seen
are given. However, some equations actually feature the same expres-
that the general relationship P ∝ cn holds true for all reference mate-
sion and only differ in the value of the empirical constant. In such a
rials. The corresponding exponents are about 1.5, which represents the
case, we treat them as one equation here. The remaining 15 equations,
value typically taken for Half-penny cracks in most references. More-
which have been examined in this work, are listed in Table 4. Generally,
over, the data points of Si (100), Si (111) and soda-lime glass all fall on
Eq. B1 to Eq. B12 were originally derived for a Half-penny crack mode
one linear relationship, while the data points of SiC (0001), sapphire
and Eq. B13 to Eq. B15 were tailored for a Palmqvist crack mode. It is
and fused quartz exhibit another linear relationship, which is shifted
noteworthy that, unlike the equations in Ponton’s work, which are
slightly upwards. The reason behind this two linear relationship phe-
summarized in chronological order, the equations in our work are re-
nomenon can be the different fracture toughness regimes the reference
arranged reflecting on their complexity. Moreover, formal similarities
materials feature, since Si (100), Si (111) and soda-lime glass feature a
are considered and the corresponding equations are bundled to facil-
relatively low fracture toughness compared to SiC (0001) and sapphire.
itate further comparison. Eq. B4 and Eq. B15 represent Anstis’s and
Notably, fused quartz’s showing up as a high fracture material is ac-
Laugier’s equations, respectively.
tually an artifact when its fracture toughness is calculated from radial
The resulting constants (for each reference material) of the 15 dif-
cracks. In fused quartz, cone-cracks are produced prior to radial cracks.
ferent equations are listed in Table 5. The errors stated in this table
Here, subsequent to the occurrence of the first cone-crack, the forma-
arise from the accuracy of the measurements of elastic modulus,
tion of new cone-cracks and the propagation of radial cracks are sup-
hardness and crack lengths c, l and a.
posed to take place simultaneously while a major part of energy is
In summary, the constants of Si (100) and Si (111) are almost
dissipated through cone-cracks. Hence, any fracture toughness value of
identical for all equations. Moreover, considering any specific equation,
fused quartz solely based on radial crack length will be dramatically
the constants of Si (100) and Si (111) are always ˜1.5 times smaller than
overestimate its fracture toughness. Consequently, the exponential re-
those of SiC (0001), indicating that the fracture behavior of Si and SiC is
lationship between P and c provides another evidence of the necessity
different, regardless of the equation used. Consequently, it is advisable
to classify the existing reference materials. Dukino argued that
to never utilize Si and SiC as reference materials for constant calibration
Table 4
Fifteen equations arranged according to their formal similarities taken from
reference [7].
Equation expression Equation number
Table 5
Resulting constants for a Berkovich indenter using the 15 different equations listed in Table 4.
Material Eq. B1 Eq. B2 Eq. B3 Eq. B4 Eq. B5 Eq. B6 Eq. B7 Eq. B8
Si (100) 0.092 ± 0.001 0.047 ± 0.001 0.031 ± 0.001 0.024 ± 0.001 0.015 ± 0.001 0.046 ± 0.001 0.092 ± 0.001 0.017 ± 0.001
Si (111) 0.093 ± 0.001 0.048 ± 0.001 0.032 ± 0.001 0.024 ± 0.001 0.016 ± 0.001 0.046 ± 0.001 0.092 ± 0.001 0.018 ± 0.001
Soda-lime glass 0.085 ± 0.002 0.046 ± 0.001 0.031 ± 0.001 0.025 ± 0.001 0.016 ± 0.001 0.028 ± 0.001 0.088 ± 0.005 0.013 ± 0.001
SiC (0001) 0.14 ± 0.01 0.071 ± 0.001 0.048 ± 0.001 0.037 ± 0.001 0.024 ± 0.001 0.067 ± 0.001 0.13 ± 0.01 0.027 ± 0.001
Sapphire 0.13 ± 0.01 0.064 ± 0.001 0.043 ± 0.001 0.032 ± 0.001 0.021 ± 0.001 0.047 ± 0.001 0.12 ± 0.01 0.020 ± 0.001
Fused quartz 0.035 ± 0.001 0.021 ± 0.001 0.015 ± 0.001 0.012 ± 0.001 0.009 ± 0.001 0.022 ± 0.001 0.038 ± 0.001 0.011 ± 0.001
Eq. B9 Eq. B10 Eq. B11 Eq. B12 Eq. B13 Eq. B14 Eq. B15
Si (100) 0.032 ± 0.001 0.59 ± 0.02 0.077 ± 0.003 0.12 ± 0.01 0.011 ± 0.001 0.034 ± 0.001 0.015 ± 0.001
Si (111) 0.033 ± 0.001 0.60 ± 0.03 0.080 ± 0.003 0.12 ± 0.01 0.012 ± 0.001 0.034 ± 0.001 0.016 ± 0.001
Soda-lime glass 0.034 ± 0.001 0.45 ± 0.02 0.068 ± 0.003 0.13 ± 0.01 0.008 ± 0.001 0.023 ± 0.001 0.023 ± 0.001
SiC (0001) 0.050 ± 0.001 0.90 ± 0.04 0.13 ± 0.01 0.20 ± 0.02 0.017 ± 0.001 0.048 ± 0.001 0.024 ± 0.001
Sapphire 0.045 ± 0.001 0.64 ± 0.07 0.081 ± 0.002 0.14 ± 0.01 0.013 ± 0.001 0.038 ± 0.001 0.027 ± 0.001
Fused quartz 0.016 ± 0.001 0.37 ± 0.03 0.12 ± 0.01 0.15 ± 0.01 0.006 ± 0.001 0.013 ± 0.001 0.006 ± 0.001
at the same time. This is also true for the case of soda-lime glass and two parts. One part is identical to Eq. B1 to Eq. B5, which, as has al-
sapphire (the constants of soda-lime glass, in most cases, except for Eq. ready been shown, follows our idea of classification. The second part is
B12 and Eq. B15, are ˜1.5 times smaller than those of sapphire). a function of m as can be seen in Table 6, which, as will be shown later
A closer look at the individual expressions of the equations reveals on, is the actual reason behind some of the irritations stated above
that Eq. B1 to Eq. B5 only contain the total crack length c, whereas, P/ concerning classification.
c3/2 is a fixed term and the exponent in (E/H)n varies from 0 to 2/3. All equations that have been proposed earlier based on various
Moreover, based on the values of the calculated constants presented in physical theories or models can be written into a universal form as
Table 5, the classification proposed here still remains reasonable. For shown in Eq. 6, where k is the empirical constant. E, H, Pmax and c are
Eq. B6 to Eq. B15, the crack length a or l is introduced, adding a higher elastic modulus, hardness, maximum indentation load and total crack
degree of complexity: length at the maximum indentation load, respectively. f(m) is a function
of m, or c to a ratio.
I) For some equations (Eq. B7, B9 and B12), Si (100), Si (111) and
Kifr = k (E/H)n Pmax/c3/2 f(m) (6)
soda-lime glass belong to the same group; while for other equations
(Eq. B6, B8, B10, B11, B13, B14 and B15), the constants indicate If f(m) is taken as unity in Eq. 6, Kifr = k (E/H) P/c n 3/2
can be
that they should not be categorized into one group. regarded as a universal form representing Eq. B1 to Eq. B5.
II) For some equations (Eq. B7, B9 and B15), SiC and sapphire belong to Accordingly, the calculated constants should meet the classification
the same group; while for others (Eq. B6, B8, B10, B11, B12, B13 Group I: Si (100), Si (111), soda-lime glass; Group II: SiC, sapphire and
and B14), the constants show that they probably should not be Group III: fused quartz, which can also be confirmed by observing
considered as members of the same group. Table 5. However, when f(m) is considered in the formulation, it seems
that the classification changes according to the values of the calculated
To shed some light on this phenomenon, subsequently, Eq. B6 to Eq. constants. Regardless of any physical implications behind these equa-
B15 will be rewritten into a new form. Since c = a + l, assuming tions, mathematically, this change is mainly due to the different re-
gimes of f(m) associated with the different reference materials. To
c/a = m, (3)
clarify the effect of different regimes, Fig. 7 displays a plot of f(m) for
then a and l are, the various equations. In our case, the m value (c/a ratio) of Si (100), Si
(111) and SiC (0001) is in the same range ranging from 1.4 to 2.0
a = c/m (4)
(grey), since the total crack length c increases more rapidly than a with
and increasing maximum load. For sapphire, m falls in the range from 2.0 to
2.5 (orange), while m shows values ranging from 2.4 to 2.8 (light blue)
l = (m-1)/m·c, (5) for soda-lime glass. Moreover, at different m regimes, f(m) is also a
respectively. constant that will have an effect on the value of the empirical constant
Inserting Eqs. 4 and 5 into Eq. B6 to Eq. B15 (replacing a and l with c k.
and m) results in a new form of Eq. B6 to Eq. B15, which is composed of Generally, an increase in f(m) in Kifr = k (E/H)n P/c3/2 f(m) will
Table 6
The new form of Eq. B6 to Eq. B15, rewritten with c and m.
Equation number Equation expression
* F = -1.59-0.34B-2.02B2+11.23B3-24.97B4+16.32B5, B = log(c/a).
#
f(E/H) = 0.75*(βEXP2/δ – 1.5), δ = 2(1 + 3lnβEXP)/3, βEXP = 0.768(E/H)0.408.
Y. Guo, et al.
Fig. 7. Graphical representation of the second part (the function of m) in Eq. B6 to Eq. B15 after replacing a and l with c and m. m ranges from 1.4 to 2.0 for Si (100),
Si (111) and SiC (0001) (grey); from 2.0 to 2.5 for sapphire (orange) and from 2.4 to 2.8 for soda-lime glass (light blue). (For interpretation of the references to colour
in this figure legend, the reader is referred to the web version of this article.)
Y. Guo, et al.
lead to a decrease in k and vice versa. Furthermore, the following ex- Therefore, for the sake of simplification, in this chapter we only focus
planations can be derived when taking the addition of f(m) in Eq. B6 to on the first two groups and discard the third group (fused quartz). One
Eq. B15 into consideration. reference material from each group was chosen to perform the FIB
experiments. In the first group, Si (100) was chosen, while in the second
I) The m regimes for Si (100), Si (111) and SiC (0001) are identical group, SiC (0001) was selected. Fig. 8 illustrates the experimental and
(from 1.4 to 2.0), thus the finding that the constants for SiC (0001) analytical procedure, including examples of images taken from the top
are always 1.5 times larger than the ones for Si (100) and Si (111) is view and cross-sectional view of some cracks.
unaffected by f(m). In this context, Fig. 8(a) gives a schematic, introducing the para-
II) In Eq. B7 and Eq. B9, despite the fact that the m regime varies for meters that are measured after one cross-section is created. Fig. 8(b)
the different reference materials, f(m) remains almost unchanged. and (e) are SEM images of the untreated cracks of Si (100) and SiC
Thus, for these equations, the calculated constants are or rather the (0001), respectively. The crack in Si (100) was created at an indenta-
classification of reference materials is hardly affected by the term f tion displacement of 680 nm and features a total crack length of 4.3 μm.
(m). The classification of the reference materials according to the The one on SiC (0001) was created at an indentation depth of 650 nm
constants values using Eq. B7 and Eq. B9 is very close to the clas- and its total crack length is about 4.4 μm. Fig. 8(c) and (f) show the
sification, which results from using Eq. B1 to Eq. B5. cross-sections of Si (100) and SiC (0001) after a clean cut, while
III) In other equations (Eq. B6, B8, B10, B11, B12, B13, B14 and B15), f Fig. 8(d) and (g) display the corresponding surface views after the cut,
(m)soda-lime glass is approximately 1.5 times larger than f(m)Si (100) respectively. The length measured from the center of the indentation
and f(m)Si (111). Therefore, in such cases, the empirical constant impression to the cross-sections ds as well as the crack length on the
calculated for soda-lime glass will be ˜1.5 times smaller than the corresponding cross-section dcs are evaluated by SEM observation and
one of Si (100) and Si (111). This statement is also applicable to the recorded. It should be noted that there can be a so called curtaining
case of sapphire and SiC. effect [29] on the cross-sections as marked by the red arrows in Fig. 8(c)
IV) It should be noted that the term [f(E/H)] in Eq. B11 and Eq. B12 is a and (d). In the case of Si (100), the crack is easily distinguishable from
material dependent constant, which further adds to the complexity the curtaining effect. However, when the curtaining effect is in line
in the calculation of the empirical constants k in those equations. with the crack, as in SiC (0001), it will add some difficulties with re-
However, the change of the calculated constants due to term [f(E/ spect to the accurate estimation of the crack length. To tackle with this
H)] still obeys a similar interrelationship as described above for f situation, images taken at higher magnification and higher contrast are
(m) and k, that an increase in [f(E/H)] will lead to the decrease of k, required. Subsequently, several cross-sections are created along a crack
and vice versa. – i.e. along the direction towards the center of the indentation induced
imprint. The lengths of ds and dcs are recorded for each cross-section,
Consequently, the classification of the six reference materials in- respectively. Finally, based on the obtained information, the crack
vestigated in this work has again been recognized/verified: Group I: Si morphology within Si (100) and SiC (0001) can be reconstructed as
(100), Si (111), soda-lime glass; Group II: SiC, sapphire; Group III: fused shown in Fig. 9.
quartz. If the materials within one group are chosen as reference ma- The colored regions in Fig. 9(a) and (b) correspond to the crack
terials, all equations should give similar results. Moreover, according to morphology in Si (100) and SiC (0001), respectively. The plots them-
our discussion, the underestimation/overestimation of fracture tough- selves are based on the measured crack lengths on several cross-sections
ness values and the non-universal applicability property of the fracture and the positions of the corresponding cross-sections. In general, the
toughness equations are both owing to the inappropriate choice of re- crack morphology in Si (100) and SiC (0001) are significantly different
ference materials. with respect to each other and, in particular, are neither ideal Half-
Although the classification of the reference materials can explain penny nor Palmqvist type in shape. The crack in Si (100) features an
many unanswered questions, the scientific reason behind such a clas- almost Half-penny shaped morphology and the deepest part of the crack
sification remains unclear. It is strongly believed that the morphology is situated at the center of the crack itself. Moreover, the ratio of crack
of the indentation induced cracks can always be identified as Half- length on the surface to crack depth is ˜1.5 for Si (100). The crack
penny or Palmqvist type. [12] Furthermore, Dukino reports, that in- morphology in SiC (0001) approximately resembles a rectangle with
denting materials featuring a low fracture toughness with a Vickers the deepest part of the crack situated directly at the center of the indent
indenter generally leads to the formation of a Half-penny crack whereas induced impression. Besides, there is quite a large, non-negligible re-
materials with a high fracture toughness typically show Palmqvist gion around the indenter free of any cracks in SiC (0001) as seen in
cracks [28]. Therefore, the actual crack morphology of the reference Fig. 9(b), which implies that the cracks start somewhere below the
materials might be the reason behind the classification. Consequently, it indent impression. Such a median crack starts possibly at the stress
is necessary to take a closer look at the crack morphology formed concentration sites featured by shear fault intersections [30], definitely
within the individual reference materials. relying on a completely different mechanism compared to the one ob-
served for Si (100).
3.3. The investigation of crack morphology In summary, the crack morphology in Si (100) and SiC (0001) dif-
fers in shape. This finding could account for the necessary classification
Within this chapter, the crack morphology of the reference materials of the reference materials. Based on these results, we propose an im-
is investigated to further work on a scientifically meaningful basis of the proved procedure to determine fracture toughness from radial cracks
classification concept. However, the difference in crack morphology induced by nanoindentation, which will be introduced in the next
(Half-penny or Palmqvist crack) within the six reference materials chapter.
cannot be distinguished by top-view SEM images. Thereby, for the
purpose of crack morphology investigation, FIB-cutting has been em- 3.4. An improved procedure to determine fracture toughness from radial
ployed to obtain several cross-sections along the cracks. It is also no- cracks by nanoindentation
teworthy that the core discussion of this chapter is about Half-penny
and Palmqvist cracks, whereas cone cracks, as in the case of fused The previous chapters highlighted the role of the choice of reference
quartz, cannot be handled with existing fracture toughness equations. materials in the context of fracture toughness evaluation by means of
Y. Guo, et al.
Fig. 8. (a) Schematic of a cross-section along the indent-induced crack; SEM images of the untreated crack of (b) Si (100) and (e) SiC (0001); the cross-sections of (c)
Si (100) and (f) SiC (0001); top view SEM images of (d) Si (100) and (g) SiC (0001) corresponding to (c) and (f).
Y. Guo, et al.
Fig. 9. Crack morphology in (a) Si (100) and (b) SiC (0001) reconstructed ac-
cording to the measured crack lengths on the cross-sections and the positions of
the corresponding cross-sections.
Fig. 12. The Pmax c−3/2 – c1/2 relationships for the nanostructured diamond/SiC
Fig. 11. Crack morphology of the nanostructured diamond/SiC composite film. composite film analyzed within this study.
The hardness and elastic modulus of the composite film used are our work, there is no professional or other personal interest of any
49.8 ± 2.1 GPa and 598 ± 7 GPa, respectively. For details, please nature or kind in any product, service and/or company that could be
refer to our previous work [19]. The error in the result stems from construed as influencing the position presented in, or the review of, the
uncertainties in the linear fitting procedure as well as in the experi- manuscript entitled “A detailed analysis of the determination of frac-
mental hardness and modulus data. ture toughness by nanoindentation induced radial cracks”.
In literatures, the fracture toughness of diamond/SiC composite
material – synthesized by reactive sintering under high pressure and Acknowledgements
high temperature conditions or sintered by a high pressure infiltration
technique are comparable to our results [34,35]. However, in those Yuning Guo gratefully acknowledges the financial support from the
references, fracture toughness is calculated based on the length of radial China Scholarship Council (Chinese Government Scholarship, Award
cracks utilizing certain equations to obtain fracture toughness. How- No. 201504910733). Part of this work was performed at the Micro- and
ever, since all potential drawbacks of the classical approach we dis- Nanoanalytics Facility (MNaF) of the University of Siegen.
cussed above have not been considered in the process of achieving the
values, a direct comparison of the values reported there and the ones References
obtained in our study has to be handled with care. Nevertheless, we are
able to support the finding of an enhanced fracture toughness of the [1] S. Palmqvist, The work for the formation of a crack during Vickers indentation as a
diamond/SiC composite film, as has already been reported for bulk measure of the toughness of hard metals, Arch. Eisenhuettenwes 33 (1962)
629–634.
diamond/SiC composites [34,35]. [2] S. Palmqvist, Indentation hardness and fracture toughness in single crystal,
Jernkontorets Ann. 141 (1957) 300–306.
4. Conclusion [3] B.R. Lawn, A. Evans, D. Marshall, Elastic/plastic indentation damage in ceramics:
the median/radial crack system, J. Am. Ceram. Soc. 63 (9–10) (1980) 574–581.
[4] G. Anstis, P. Chantikul, B.R. Lawn, D. Marshall, A critical evaluation of indentation
In this work, a thorough examination of the existing fracture techniques for measuring fracture toughness: I, direct crack measurements, J. Am.
toughness equations has been carried out utilizing six common re- Ceram. Soc. 64 (9) (1981) 533–538.
[5] M. Laugier, Palmqvist indentation toughness in WC-Co composites, J. Mater. Sci.
ference materials (Si (100), Si (111), soda-lime glass, SiC (0001), sap-
Lett. 6 (8) (1987) 897–900.
phire and fused quartz). The choice of appropriate reference materials [6] M. Laugier, New formula for indentation toughness in ceramics, J. Mater. Sci. Lett.
was identified as crucial key to obtain scientifically meaningful and 6 (3) (1987) 355–356.
[7] C.B. Ponton, R.D. Rawlings, Vickers indentation fracture toughness test Part 1
reproducible results. Furthermore, the classification of the reference
Review of literature and formulation of standardised indentation toughness equa-
materials into three groups is proposed: Group I: Si (100), Si (111) and tions, Mater. Sci. Technol. 5 (9) (1989) 865–872.
soda-lime glass; Group II: SiC and sapphire; Group III: fused quartz. A [8] G.D. Quinn, R.C. Bradt, On the Vickers indentation fracture toughness test, J. Am.
Focus ion beam study proved that the basis of this classification could Ceram. Soc. 90 (3) (2007) 673–680.
[9] G.D. Quinn, Fracture toughness of ceramics by the Vickers indentation crack length
be related to the actual crack morphology – Si (100) in Group I features method: a critical review, Ceramic Engineering and Science Proceedings (2007) 45.
an almost Half-penny shaped morphology while the cracks in SiC [10] R. Morrell, Fracture toughness testing for advanced technical ceramics: inter-
(0001) in Group II display nearly a rectangle type of morphology. The nationally agreed good practice, Adv. Appl. Ceram. 105 (2) (2006) 88–98.
[11] D.B. Marshall, R.F. Cook, N.P. Padture, M.L. Oyen, A. Pajares, J.E. Bradby,
actual crack morphology of the reference materials differs strongly from I.E. Reimanis, R. Tandon, T.F. Page, G.M. Pharr, The compelling case for indenta-
the ideal Half-penny or Palmqvist assumptions made by the corre- tion as a functional exploratory and characterization tool, J. Am. Ceram. Soc. 98 (9)
sponding models. Moreover, all equations typically utilized in the (2015) 2671–2680.
[12] K.I. Schiffmann, Determination of fracture toughness of bulk materials and thin
context of fracture toughness evaluation have been shown to yield films by nanoindentation: comparison of different models, Philos. Mag. 91 (7-9)
equally valid results as long as appropriate reference materials are (2011) 1163–1178.
chosen. Based on these results, an improved procedure to determine [13] C. Ponton, R. Rawlings, Vickers indentation fracture toughness test Part 2
Application and critical evaluation of standardised indentation toughness equa-
fracture toughness has been proposed. Nevertheless, it should be tions, Mater. Sci. Technol. 5 (10) (1989) 961–976.
pointed out that this improved procedure proposed in this work is for [14] G. Pharr, D. Harding, W. Oliver, Measurement of Fracture Toughness in Thin Films
better accuracy in fracture toughness measurements by nanoindenta- and Small Volumes using Nanoindentation Methods, Mechanical Properties and
Deformation Behavior of Materials Having Ultra-Fine Microstructures, Springer,
tion and is valid only under specific background researches (e.g. ex-
1993, pp. 449–461.
tensive study of the crack behavior and crack morphology of a variety [15] N. Cuadrado, J. Seuba, D. Casellas, M. Anglada, E. Jiménez-Piqué, Geometry of
of reference materials). Moreover, none of the existing equations is nanoindentation cube-corner cracks observed by FIB tomography: implication for
recommended for better universality. Finally, with the help of this fracture resistance estimation, J. Eur. Ceram. Soc. 35 (10) (2015) 2949–2955.
[16] N. Cuadrado, D. Casellas, M. Anglada, E. Jiménez-Piqué, Evaluation of fracture
improved method, the fracture toughness of a diamond/SiC composite toughness of small volumes by means of cube-corner nanoindentation, Scr. Mater.
film has been successfully estimated and an enhanced fracture tough- 66 (9) (2012) 670–673.
ness of 11.1 ± 1.1 MPa·m1/2 was observed for this film material. [17] W.C. Oliver, G.M. Pharr, An improved technique for determining hardness and
elastic modulus using load and displacement sensing indentation experiments, J.
Aside from an improved procedure to estimate fracture toughness Mater. Res. 7 (6) (1992) 1564–1583.
with increased accuracy, the importance of this work also lies in its [18] F. Richter, M. Herrmann, F. Molnar, T. Chudoba, N. Schwarzer, M. Keunecke,
capability to answer some of today’s open questions in indentation K. Bewilogua, X. Zhang, H.-G. Boyen, P. Ziemann, Substrate influence in Young’s
modulus determination of thin films by indentation methods: cubic boron nitride as
based fracture toughness analysis. Here it was possible to show that the an example, Surf. Coat. Technol. 201 (6) (2006) 3577–3587.
reason for the issue of the nonexistence of a universal equation to [19] Y. Guo, T. Staedler, H. Fu, S. Heuser, X. Jiang, A novel way to quantitatively de-
calculate fracture toughness as well as issues occurring in context of termine the mechanical properties of thin films from the initial-grown surface by
nanoindentation, Appl. Surf. Sci. 479 (2019) 253–259.
under- or overestimated fracture toughness values could be tracked [20] R.F. Cook, G.M. Pharr, Direct observation and analysis of indentation cracking in
back to an inappropriate choice of reference materials. Consequently, glasses and ceramics, J. Am. Ceram. Soc. 73 (4) (1990) 787–817.
this work represents new promising guidelines/criterions to re- [21] R. Hull, Properties of Crystalline Silicon, IET, 1999.
[22] G. Žagar, V. Pejchal, M.G. Mueller, L. Michelet, A. Mortensen, Fracture toughness
producibly determine fracture toughness based on indentation induced
measurement in fused quartz using triangular chevron-notched micro-cantilevers,
radial cracks. Scr. Mater. 112 (2016) 132–135.
[23] M.M. Wood, J. Weidlich, Empirical evaluation of fracture toughness: the toughness
Declaration of Competing Interest of quartz, Am. Mineral. 67 (9–10) (1982) 1065–1068.
[24] D.J. Morris, R.F. Cook, In situ cube-corner indentation of soda–lime glass and fused
silica, J. Am. Ceram. Soc. 87 (8) (2004) 1494–1501.
The Authors claim non-conflicts of interests. [25] R.F. Cook, Ph. D Thesis. University of New South Wales, Sydney, NSW, Australia,
We declare that we have no financial and personal relationships (1986).
[26] F. Ebrahimi, L. Kalwani, Fracture anisotropy in silicon single crystal, Mater. Sci.
with other people or organizations that can inappropriately influence
Y. Guo, et al.
Eng. A 268 (1–2) (1999) 116–126. [32] J.B. Davis, J.P. Löfvander, A.G. Evans, E. Bischoff, M.L. Emiliani, Fiber coating
[27] J.-i. Jang, G. Pharr, Influence of indenter angle on cracking in Si and Ge during concepts for brittle-matrix composites, J. Am. Ceram. Soc. 76 (5) (1993)
nanoindentation, Acta Mater. 56 (16) (2008) 4458–4469. 1249–1257.
[28] R.D. Dukino, M.V. Swain, Comparative measurement of indentation fracture [33] J. Malzbender, G. De With, Elastic modulus, hardness and fracture toughness of
toughness with Berkovich and Vickers indenters, J. Am. Ceram. Soc. 75 (12) (1992) SiO2-filled methyltrimethoxysilane coatings on glass substrates, J. Non. Solids 265
3299–3304. (1–2) (2000) 51–60.
[29] P.R. Munroe, The application of focused ion beam microscopy in the material sci- [34] Y. Zhao, J. Qian, L.L. Daemen, C. Pantea, J. Zhang, G.A. Voronin, T.W. Zerda,
ences, Mater. Charact. 60 (1) (2009) 2–13. Enhancement of fracture toughness in nanostructured diamond–SiC composites,
[30] B.R. Lawn, R.F. Cook, Probing material properties with sharp indenters: a retro- Appl. Phys. Lett. 84 (8) (2004) 1356–1358.
spective, J. Mater. Sci. 47 (1) (2012) 1–22. [35] G. Voronin, T. Zerda, J. Gubicza, T. Ungár, S. Dub, Properties of nanostructured
[31] D.B. Marshall, B.R. Lawn, An indentation technique for measuring stresses in diamond-silicon carbide composites sintered by high pressure infiltration tech-
tempered glass surfaces, J. Am. Ceram. Soc.-Discussions Notes 60 (1–2) (1977) nique, J. Mater. Res. 19 (9) (2004) 2703–2707.
86–87.