You are on page 1of 4
Lean /WFPS LDA, aa DESCON ENGINEERING LTD. REPORT ON CONCRETE MIX DESIG! AASHTO 727-93 (ASTM C136-64a) ev No Date aye N ‘Doc: No|-GAROGFRW oO Feb 16,2007 vort pect No: SaoB Ae 4 2 Of Material: SAAU/ SAtore srthenmmoel. QIPNo.on4 erlal Supplied £04 § Requicement innary Tess Project Name: Ladnse 2a ae Sample No: 7 Lab. Ret. No. [Cement ]Fine Aggregate/Sand [Coarse Aggregate D.G GRO) | sae pr pear [KasmoreiSakhi Sarwar I ‘Admixture? Slump’ = Y [28 days cylinder strength 228 C-Class [Sp. Gravy [Absorption Sieve nit Weight (kgind) [SSD basis [% Dry Roddes Loose ree Aggregate "7 [Annaxad Zs Sto | AF 2 yegale SAen! SAgwAR Ze3 [Annexed E z = sngth Consideration Mix is designed in accordance with ACI we the required strength for safety purpose. Proportions 211.1, The 28 days cylinder strength was taken about 26% to 35% [Cement Fine regate Kain’ Coarse Aggregate, Kyi [Ramiaure er Kats gm [600 mi100 Kg [IOS | 205 3S hE Mee apertios of fresh concrete trial mix Ratio [Slump (mm) lair 96 [Enirapped [Unit Weight |Temperepp ‘Comp strength 6°0°12" cylinder psi Kgrna [Says [7 days [28 Days 27o 23 Zz 2962 fe Ratio by Weight (Cement Ka| Fine Aggregate Kg Coarse Ag regate, KG a [az fc Ratio by Volume [Cement Gill Fine Aggregate Gi Coarse Ag egate, Cl “Assuming Cement bag = 50Kg = 1.25 ch PREPARED BY DESCON GARaC ENGINEER'S REPRESENTATIVE nme: GMMR, Ac He wane hr Mad emcd Poa = fiw A Moma HEY 3 Lp— Dow pate, 03-04 - deo? ore O2.4_ oF souarure Gon je. SIGNATURE: SIGNATURE: Conciete Blocks z Doe no aoorran DESCON ENGINEERING LTD. Be Oey REPORT ON CONCRETE MIX DESIGN Page Aare a AASHTO 127-93 (ASTM C136-84a) feetNo: S098 Project Name: adreee Corre C pice of Material Sample No: Zaz pos” {IP No. 004 Lab. Ret No DE 20/8 erial Supplied [Cement [Fine Aggregate/Sé Coarse Aggregate, BG (SRO) | C-7Z/4 AnD [Kasmore/Sakhi Sarwar Admisture: Requirement [Slump [BB days oylinder strength stomp 0 Class Bl inary Tests sea Sp. Gray [Absorsion [OAR Weg Rana fe [SSD basis _|% [Dry Rodded Loose eAggregate’f + Ya dD [Annexed 735 L3LO 4340. curegate lAnnexed 2s ‘a | Zssr git Consideration Ma designed in accordance with ACI 211.1. The 28 days ender srength was taken about 25% to 95% pre the required slrength for safety purpose Proportions rons, RTT ie area Kins Coates Aggregate, gin [Ramiare Kats 00 mi0OKe 132 o 330 sao + [750 L250 pperes of fresh concrete wal mie — Peat [Slump tri) entrapped [Unk Weight’ |Temperapp | ——Comptrengih 0°12" eyindsr psi Jac [Kgims days [Fdays [28 Days oO ro Zz 2432_| 27 = a by Weight (Gementka] Fine Aggregate Ke Coarae Agaregate, Kg We SSS masss |e see 37 fs Roto by Volume (Cement. Ci] Fine Aogregate GF Coarse Aggregate, CH Z 37 r “Assuming Cement bag = 50Kg = 1.25 Cit PREPARED BY esconaagac ENGINEERS REPRESENTATIVE " Gibiook A CheenA we, Sh Madea foutude | wa ve Likes A - Ofer Re gang 2207 f i Quo) oe gh 4 — ant eee me ey pfe J ssonaTURE Bey DN Dee No GAROCIFRM DESCON ENGINEERING LTD. SRP iby REPORT ON CONCRETE MIX DESIGN wo dae AASHTO 127-83 (ASTM C136-84a) Project Name:: Raves canal Burco of Material <5 AA 374.oodR Sample No: 7741 ord BFP No. 004 Lab, Ret Nay 2. | eel Supplied [Comert [Fine Aggregate/Sand_~ [Coarse Aggregate 7 DG (SRO) | axe aauens AR —|Kasmore/Sakhi Sarwal i Admixture; T fs Requirement [Slump [28 days cjinder stengh er Bas0 PS? iminary Tests Seve (Se: Graviy_ [Absorption [Un Weight earmay ] [SSD basis | [ry Rocded|toose q fagregele 2 D a Zas_|/s72 | ago J iehgweusle Ska Aaiak —\Nmeed —| 2 ee [2 2752 SSS q a ifength Consideration Phe Nixis designed in accordance wih ACI 211.1. The 28 days eylinder strength was taken about 25% to 35% ove the required strength for safely purpose. [Cement [Fine Aggregate Kain Coarse Aggregate, Kgind —JAdminture ] Kama Scaeuée UD [500 mir00 Re Bz 2 [DE Camp TToTal| 35 oF fresh comerate tial mit Stine (vm) [Entrepped [Uni Weight Fempore pp Comp.sirengih 6°01" oyinder pal airs Ikgima Says [7 days [25 Days [22 = 2320_| 27 - is Rat by Weight (CementKg| Fine Ragregate Ka Coarse Aggregate. KG ~ SSaawar TD L2r3 SUG — Foo | 2 34 Wee Rao by Volume [Cement,CR] Fine Aggregate oft Coarse Aggregale, Cit i. TD 7 Eee | EIS Za = ww Live 2-2. 3.357 * Assuming Cement bag = 50Kg = 1.25 0h PREPARED aY DESCOW aAKOC ENGINEERS REPRESENTATIVE none: SE Aba) occ | nae Ai fee 03 - A0e7 1 29-03-2007, [me 28-03 7 on A, ale sonarus 73 fa SIGNATURE: SY Dea to dawaoiran DESCON ENGINEERING LTD. ee ee REPORT ON CONCRETE MIX DESIGN oe AASHTO 127-93 (ASTM C136-84a) jetNo Sook ey Project Name anes Camel utc of Material: Sgucnls SA/CIIAR Sample No.0 -094 Lab. Ref NoDL 0/5 [Camant Fine Aggragate/Sand [Coarse Aggregate DG (SRC) piod —|KasmorelSakhi Sarwat 7 ‘Admixture? [Slump [28 days cylinder strength = (aaa PS? A ins sieve [Sp. Gravity [Absorption [Unit Weight (kaima) | SSD basis _|% [Dry RoddedLoose | 7D lannexed 3 1 ABs 3% | SARIGAR—|Armexed Zso | Zsa 1 igi Consideration . fie Mixis designed in accordance with ACI 211.1. The 28 days cjinder strength was taken about 25% to 35% jove the required strenath for safely purpose. fix Proportions eter Kom Cement Fine Aggregate Kgims Coarse Aggregate, Kgims —JAdmisture 7 cgi EXIEeTIe 4D [600 mv100 Kg = CLE opertios of fresh concrete trial mix {Slump (mm) [entrapped [Unt Weight Temperepp Comp strength 6°0"12" cylinder psi airs [kgima Saas [7days [2 Days 72 cE 100 7 Bysb | pga |3t" Vai Ral by Weigh [Cementikg| Fine Aggregate Ko Gaarce Aggregate, Kg Pana A123. zZ Ratio by Volume [Cement.CR] Fine Aggregate Of Coarse Aggiegate, Gh LD ~ 3 “3. Assuming Cement bag = S0Kg = 1.25 Cit PREPARED BY DESCON aAsaC ENGINEERS REPRESENTATIVE Clk hcteene we (Mouse /— we i A Te WEQ3- 93—2o0 pate: 29--ol,— Dev] we 2o- wf OE = Wey *

You might also like