Professional Documents
Culture Documents
1DQRLQGHQWDWLRQ
+=KDQJ*7:*RK<+XDQJ
$SSOLHG0DWHULDOV
$
67$5,QVWLWXWHRI0DWHULDOV5HVHDUFKDQG(QJLQHHULQJ
8QLYHUVLW\RI&DPEULGJH
$SSOLHG0DWHULDOV6LQJDSRUH7HFKQRORJLHV3WH/WG
6FLHQFH3DUN5G%7KH$OSKD6FLHQFH3DUN,,
6LQJDSRUH
+DQZHQB=KDQJ#DPDWFRP
$EVWUDFW 7KHRU\
7KLV SDSHU ZKLFK LV EDVHG RQ D SURMHFW EHWZHHQ $SSOLHG &RPPRQ H[SHULPHQWDO PHWKRGV WR FKDUDFWHUL]H IUDFWXUH
0DWHULDOV DQG WKH ,QVWLWXWH RI 0DWHULDOV 5HVHDUFK DQG WRXJKQHVV LQFOXGH WKH WKUHHSRLQW EHQGLQJ WHVW DQG
(QJLQHHULQJ ,05( GHVFULEHV D QRYHO PHWKRGRORJ\ WR QDQRLQGHQWDWLRQ >@ )RU 6L1 WKLQ ILOPV RI WKLFNQHVVHV RI
FKDUDFWHUL]HWKHIUDFWXUHWRXJKQHVVRIVLOLFRQQLWULGH6L1WKLQ DERXWȝPDQGEHORZGHSRVLWHGRQVLOLFRQVXEVWUDWHLWZLOOEH
ILOPVGHSRVLWHGDWXOWUDORZWHPSHUDWXUHVRI&E\WKH H[WUHPHO\ GLIILFXOW DQG FRVWO\ WR FUHDWH IUHHVWDQGLQJ ILOPV WR
3ODVPD (QKDQFHG &KHPLFDO 9DSRXU 'HSRVLWLRQ 3(&9' FRQGXFW EHQGLQJ WHVWV 7KXV WKH QDQRLQGHQWDWLRQ PHWKRG ZDV
PHWKRG 6L1 WKLQ ILOPV ZHUH GHSRVLWHG XQGHU YDU\LQJ FKRVHQZKHUHDFXEHFRUQHULQGHQWDWLRQZDVPDGHRQWKHILOP
FRQGLWLRQV WKLFNQHVV GHSRVLWLRQ WHPSHUDWXUH DQG SODVPD VXUIDFHWRSURGXFHGHILQHGFUDFNOLQHVDVLOOXVWUDWHGLQ)LJXUH
SRZHU RQ VLOLFRQ VXEVWUDWHV XVLQJ $SSOLHG 0DWHULDOV¶ &XEHFRUQHU LQGHQWHUV ZHUH VHOHFWHG DV WKHLU JHRPHWU\
352'8&(5 $YLOD70 3(&9' FKDPEHU DQG FKDUDFWHUL]HG DOORZVWKHPWRJHQHUDWHKLJKHUVWUHVVHVDWWKHLUWLSV7KXVWKH\
XVLQJ WKH QDQRLQGHQWDWLRQ PHWKRG IRU IUDFWXUH WRXJKQHVV ZHUHPRVWVXLWHGWRLQGHQWLQJWKLQILOPVZKHUHWKHLQGHQWDWLRQ
YDOXHV 7KH QDQRLQGHQWDWLRQ PHWKRG ZDV RSWLPL]HG IRU WKH GHSWKVZHUHOLPLWHG)URPWKHPD[LPXPLQGHQWDWLRQIRUFHDQG
XOWUDORZ WHPSHUDWXUH 3(&9' 6L1 ILOPV ZKLFK SURGXFHG FUDFNOLQHV¶OHQJWKIUDFWXUHWRXJKQHVVFDQEHFDOFXODWHGEDVHG
FRQVLVWHQW UHVXOWV WKDW HQDEOHG EHWWHU XQGHUVWDQGLQJ RI WKH RQDWDLORUHGPRGHO
PHFKDQLFDOSURSHUWLHVRIXOWUDORZWHPSHUDWXUH6L1ILOPV
,QWURGXFWLRQ
$PRUSKRXV GLHOHFWULF WKLQ ILOPV VXFK DV VLOLFRQ QLWULGH
6L1 GHSRVLWHG E\ WKH 3ODVPD (QKDQFHG &KHPLFDO 9DSRXU
'HSRVLWLRQ 3(&9' PHWKRG DUH FRPPRQO\ XVHG LQ WKH
VHPLFRQGXFWRU LQGXVWU\ DV GLHOHFWULF OD\HUV ,Q SDFNDJLQJ
DSSOLFDWLRQV VXFK DV ',& 7KURXJK 6LOLFRQ 9LD 769
%DFNVLGH 9LD 5HYHDO SURFHVV ZKHUH D WLJKW WKHUPDO EXGJHW
H[LVWVWKHGHSRVLWLRQRIVLOLFRQQLWULGH6L1ILOPVDWDQXOWUD
ORZWHPSHUDWXUHRI&LVUHTXLUHG&RPSDUHGWRWKHLU
KLJK WHPSHUDWXUH FRXQWHUSDUWV W\SLFDOO\ GHSRVLWHG DW DERYH )LJ6FKHPDWLFLOOXVWUDWLRQRIDFXEHFRUQHULQGHQWDWLRQRQ
& XOWUDORZ WHPSHUDWXUH ILOPV PD\ KDYH YHU\ GLIIHUHQW DILOPSURGXFLQJFUDFNOLQHVH[WHQGLQJIURPWKHYHUWLFHV
FKDUDFWHULVWLFV LQ WHUPV RI FKHPLFDO FRPSRVLWLRQ DQG
PHFKDQLFDO SURSHUWLHV 7KH XQGHUVWDQGLQJ RI WKH PHFKDQLFDO 0RGHOV GHVFULELQJ LQGHQWDWLRQ FUDFN SURSDJDWLRQ LQ ILOPV
SURSHUWLHVRIVXFKILOPVLVOLPLWHGE\WKHODFNRISULRUVWXGLHV WR FDOFXODWH ILOP IUDFWXUH WRXJKQHVV KDYH EHHQ FRQVLGHUDEO\
WKDW VSHFLILFDOO\ FKDUDFWHUL]H WKH IUDFWXUH WRXJKQHVV RI XOWUD VWXGLHG+RZHYHULQFRQWUDVWWRWKRVHGHYHORSHGE\$QVWLVHW
ORZ WHPSHUDWXUH 3(&9' 6L1 WKLQ ILOPV GHSRVLWHG RQ 6L DO >@ DQG /DXJLHU >@ ZKLFK LQYROYH KDOI
VXEVWUDWHV 7KXV LQ WKLV VWXG\ D UREXVW PHWKRGRORJ\ ZDV SHQQ\ UDGLDO DQG 3DOPTYLVW FUDFNV UHVSHFWLYHO\ )LJXUHV
GHYHORSHG WR V\VWHPDWLFDOO\ FKDUDFWHUL]H WKH IUDFWXUH DFKDQQHOFUDFNPRUSKRORJ\PRGHOGHYHORSHGE\-XQJNHW
WRXJKQHVV RI XOWUDORZ WHPSHUDWXUH 3(&9' 6L1 ILOPV EDVHG DO >@ ZDV DGRSWHG LQ WKLV VWXG\ ZKLFK LV PRUH
RQ WKH QDQRLQGHQWDWLRQ PHWKRG :LWK WKLV PHWKRGRORJ\ VXLWDEOHIRUPHFKDQLFDOO\WKLQILOPV
GHYHORSHG PHFKDQLFDO SURSHUWLHV RI XOWUDORZ WHPSHUDWXUH
6L1 ILOPV FDQ EH EHWWHU XQGHUVWRRG DQG WXQHG WR DYRLG
PHFKDQLFDOIDLOXUHVVXFKDVFUDFNLQJDQGGHODPLQDWLRQLQWKHLU
DSSOLFDWLRQV
978-1-5090-4369-9/16/$31.00 2016
c IEEE 217
3ODVWLF=RQH F
.LQGLVGHILQHGDVWKHVWUHVVLQWHQVLW\IDFWRUDWWKHFUDFNWLS
GXH WR WKH LQGHQWDWLRQ SURFHGXUH DQG LV UHSUHVHQWDWLYH RI WKH
WRWDOVWUHVVWKDWFDQEHLQGHQWHGLQWRWKHILOP7KHFRQWULEXWLRQ
&UDFN WI GXH WR WKH UHVLGXDO ILOP VWUHVV LV WDNHQ FDUH RI E\ WKH VHFRQG
6L1)LOP WHUPRI(TXDWLRQZKLFKZHVKDOOFDOO.ILOP
6XEVWUDWH భ
ܭ ൌ ߰ߪோ ܿ మ
)LJ6FKHPDWLFLOOXVWUDWLRQRIDKDOISHQQ\UDGLDOFUDFN
PRUSKRORJ\ ([LVWLQJOLWHUDWXUHKDVVKRZQWKDWLVWKHDSSURSULDWH
Į YDOXH WR XVH IRU FXEHFRUQHU LQGHQWHU WLSV ZKLOH LV
3ODVWLF=RQH F
XVHGIRUȥ>@
0HWKRGRORJ\
&UDFN &UDFN WI 6L1 ILOPV ZHUH GHSRVLWHG XVLQJ $SSOLHG 0DWHULDOV¶
352'8&(5 $YLOD70 3(&9' FKDPEHU RQ LQFK VLOLFRQ
6L1)LOP
6XEVWUDWH ZDIHUVZLWKVLODQH6L+DQGDPPRQLD1+SUHFXUVRUVLQD
QLWURJHQ HQYLURQPHQW ZLWK UDGLR IUHTXHQF\ 5) SODVPD
)LJ6FKHPDWLFLOOXVWUDWLRQRID3DOPTYLVWFUDFN 0+]7KHUHDFWLRQIRUPXODLVDVVKRZQEHORZ
PRUSKRORJ\ ோி
ܵ݅ܪସ ܰܪଷ ሱሮ ܵ݅ܰ௫ ܪ௬ ܪଶ
$V VKRZQ LQ )LJXUHV DQG WKH SODVWLF ]RQHV LQ UDGLDO 7KH 5) SRZHU DQG GHSRVLWLRQ WLPH ZHUH YDULHG WR FUHDWH
DQG 3DOPTYLVW FUDFNV DUH KHPLVSKHULFDO YROXPHV FRQWDLQHG 6L1 ILOPV RIGLIIHUHQWWKLFNQHVVHVDQG VWUHVVDQGGHSRVLWLRQV
ZLWKLQ WKH ILOPV +RZHYHU WKH ILOPV XVHG LQ WKLV VWXG\ ZHUH ZHUHGRQHDWWHPSHUDWXUHVRI&&&DVGHWDLOHG
YHU\ WKLQ ± ȝP DQG WKXV WKH FUDFN DQG SODVWLF ]RQH LQ WKH 'HVLJQ RI ([SHULPHQW 'R( SODQ LQ 7DEOH +LJK
ZHUHUHDVRQHGWRKDYHPRVWOLNHO\H[SDQGHGWKURXJKWKHHQWLUH WHPSHUDWXUH 6L1 ILOPV ZHUH DOVR GHSRVLWHG XVLQJ DQRWKHU
WKLFNQHVV RI WKH ILOP XQWLO LW UHDFKHG WKH ILOPVXEVWUDWH $SSOLHG 0DWHULDOV¶ 3(&9' FKDPEHU DW & DV D
LQWHUIDFH :LWK WKH 6L VXEVWUDWH KDYLQJ YHU\ GLIIHUHQW FRPSDULVRQIRUIUDFWXUHWRXJKQHVVFKDUDFWHUL]DWLRQ
PHFKDQLFDO SURSHUWLHV IURP WKH 6L1 ILOP DQG DVVXPLQJ WKDW
WKHUH ZDV QRGHODPLQDWLRQRIWKH ILOPIURPWKH VXEVWUDWHWKH 7DEOH'R(3ODQ
FUDFN DQG SODVWLF ]RQH ZRXOG EH OLPLWHG LQ VL]H E\ WKH &RXSRQ 7KLFNQHVVc 5) 'HSRVLWLRQ
LQWHUIDFHWRIRUPDF\OLQGULFDOYROXPHYHUVXVDKHPLVSKHULFDO 1R 3RZHU 7HPSHUDWXUHƕ&
RQH7KLVSURGXFHVDFKDQQHOFUDFNDVVKRZQLQ)LJXUH
/RZ
F N
+LJK
&UDFN &UDFN
WI
3ODVWLF=RQH
6L1)LOP /RZ
6XEVWUDWH
)LJ6FKHPDWLFLOOXVWUDWLRQRIDFKDQQHOFUDFN N
+LJK
-XQJN¶V PRGHO DVVXPHV D FKDQQHO FUDFN ZLWKRXW DQ\ /RZ
GHODPLQDWLRQ RI WKH ILOP IURP WKH VXEVWUDWH )UDFWXUH +LJK
WRXJKQHVV.FFDQEHFDOFXODWHGZLWKKLVIRUPXOD
భ
భ
ܭ ൌ
ா య ଵ
ߙቀ ቁ ൬ ൰ భ ߰ߪோ ܿ
మ $ FP [ FP FRXSRQ ZDV FXW RXW IURP HDFK ZDIHU DQG
ு ௧
మ HDFK RI WKHVH FRXSRQV ZDV LQGHQWHG WLPHV IRU IUDFWXUH
ZKHUHĮLVDFRQVWDQWIRUWKHFXEHFRUQHULQGHQWHUWLSXVHG( WRXJKQHVV FKDUDFWHUL]DWLRQ 7KH LQGHQWDWLRQV ZHUH SHUIRUPHG
LV WKH <RXQJ¶V PRGXOXV + LV WKH KDUGQHVV WI LV WKH ILOP ZLWK WKH $JLOHQW 1DQR ,QGHQWHU * HTXLSSHG ZLWK WKH ;3
WKLFNQHVV3LVWKHPD[LPXPLQGHQWDWLRQ IRUFH FLVWKHFUDFN KHDG7KH1DQR,QGHQWHU*LVSRZHUHGE\HOHFWURPDJQHWLF
OHQJWK ȥ LV D SDUDPHWHU UHODWHG WR WKH 'XQGXUV¶ SDUDPHWHUV DFWXDWLRQEDVHG IRUFH WUDQVGXFHUV ZLWK D ORDG UHVROXWLRQ RI
DQGı5LVWKHUHVLGXDOILOPVWUHVVLQKHUHQWLQD3(&9'ILOP Q1DQGLWLVDOVRFDSDEOHRID ]GLVSODFHPHQWUHVROXWLRQ RI
(TXDWLRQFDQEHYLHZHGDVDVXSHUSRVLWLRQRIWZRSDUWV QP 7KLV JLYHV LW WKH DELOLW\ WR SURGXFH DFFXUDWH DQG
WKDW WDNH LQWR DFFRXQW ERWK LQGHQWDWLRQ VWUHVV DQG RXU ILOPV¶ UHSHDWDEOHPHDVXUHPHQWV$FXEHFRUQHULQGHQWHUWLSZDVXVHG
UHVLGXDO VWUHVV WKH ODWWHU RI ZKLFK KDV EHHQ NQRZQ WR DVLWKDVEHWWHUIRUFHFRQFHQWUDWLRQIRUWKHFUDFNLQWURGXFWLRQ
VLJQLILFDQWO\ DIIHFW IUDFWXUH WRXJKQHVV FDOFXODWLRQV >@ )LUVW 7KH LQGHQWDWLRQ ZDV GRQH RQ WKH FRXSRQV WR WKH GHSWK LQ
WKHDSSDUHQWIUDFWXUHWRXJKQHVV.LQGLVFDOFXODWHGE\ DFFRUGDQFH WR WKH WKLFNQHVV RI WKH 6L1 ILOP NcNc WR
భ LQWURGXFHFUDFNVLQWKHILOPVDQGWRKDYHDIL[HGSDUDPHWHUIRU
ா య ଵ
ܭௗ ൌ ߙ ቀ ቁ ൬ ൰ భ WKHWHVW7KHPD[LPXPLQGHQWDWLRQIRUFH3ZDVUHFRUGHGIRU
ு ௧
మ IUDFWXUHWRXJKQHVVPHDVXUHPHQWV
3P1
OHQJWKVIRUWKDWSDUWLFXODULQGHQWDWLRQ¶VFYDOXH
$VDUHVXOWWKHQXPEHURIVXFFHVVIXOLQGHQWDWLRQVQPDGH
RQHDFKFRXSRQYDULHGIURPWRLQGHQWDWLRQV
'LVSODFHPHQWQP
)LJ/RDGGLVSODFHPHQWFXUYHVRIWKHVXFFHVVIXO
LQGHQWDWLRQVLQ&RXSRQ
)LJXUH VKRZV D IHZ H[DPSOHV RI WKH FUDFN OHQJWKV
PHDVXUHGXQGHU6(0LPDJLQJ
)LJ$Q,QGHQWDWLRQIURP&RXSRQWKDWGLGQRWSURGXFH
FUDFNOLQHV6XUIDFHVSXWWHUHGZLWKJROG
)LJ)URPOHIW6(0LPDJHVRIFUDFNOHQJWKVIURP
LQGHQWDWLRQVLQNcƕ&ƕ&DQGƕ&FRXSRQV7KH
ƕ&LQGHQWDWLRQLVDQH[DPSOHRIRQHZLWKRQO\YLVLEOH
FUDFNVIURPWKHYHUWLFHV
$Q DYHUDJH RI WKH FUDFN OHQJWKV ZHUH WDNHQ IURP HDFK
LQGHQWDWLRQ EHIRUH WKH FUDFN OHQJWK IRU WKDW FRXSRQ ZDV
GHWHUPLQHG ZLWKDQDYHUDJHRIWKH IRUPHUYDOXHV7KHUHVXOWV
DUHGHWDLOHGEHORZLQ7DEOH
8VLQJ(TXDWLRQWKH IUDFWXUHWRXJKQHVVZDVFDOFXODWHG
IRUHDFKLQGHQWDWLRQEHIRUHDQDYHUDJHZDVWDNHQWRREWDLQWKH
)LJ$QLQGHQWDWLRQIURP&RXSRQWKDWVKRZHG IUDFWXUH WRXJKQHVV RI HDFK ILOP 7KH UHVXOWV ZHUH WDEXODWHG
XQGHVLUDEOHGDPDJHWRWKHILOP WRJHWKHU LQ 7DEOH DQG SORWWHG DJDLQVW WKH WHPSHUDWXUH IRU
HDFK 5) SRZHU VHWWLQJ LQ )LJXUH 7KH HUURU EDUV UHSUHVHQW
WKUHHWLPHVWKHVWDQGDUGHUURULQPHDQ
Nc+LJK3RZHU Nc/RZ3RZHU
Nc/RZ3RZHU Nc+LJK3RZHU
Nc &/RZ3RZHUNcƕ&+LJK3RZHU
ƕ
Position of FIB
cross-section
.F03D¥P
)LJ&XWZKHUH),%ZDVWDNHQIURP6KRZQ,QGHQWDWLRQ
RQ&RXSRQ
Platinum
Coupon Surface
«« SiN Film
7HPSHUDWXUHƕ&
)LJ*UDSKRI.FDJDLQVW7HPSHUDWXUH Substrate
7R YHULI\ WKH FUDFN PRUSKRORJ\ D IHZ LQGHQWDWLRQV ZHUH
VHOHFWHGIRUFURVVVHFWLRQLPDJLQJXVLQJWKHIRFXVHGLRQEHDP
),%DVVKRZQLQ)LJXUHVWR
)LJ),%&URVVVHFWLRQRI&RXSRQ
Coupon Surface
SiN Film
S3
S2
S2 Substrate
S1
S1
)LJ&XWVPDGHRQDQLQGHQWDWLRQRQ&RXSRQIRU),% )LJ)URPWRS),%FURVVVHFWLRQDWSRVLWLRQV66DQG
6UHVSHFWLYHO\
5HVXOWVDQG'LVFXVVLRQ
6WDWLVWLFDOO\WKHSHUFHQWDJHHUURUVLQWKHUHVXOWV ZHUHORZ
Platinum
VKRZLQJ WKH FRQVLVWHQF\ RI WKH QDQRLQGHQWDWLRQ
Coupon Surface PHWKRG WKDW ZH KDG RSWLPL]HG 7KH UHVXOWV VKRZHG WKDW WKH
IUDFWXUH WRXJKQHVV RI $SSOLHG 0DWHULDOV¶ XOWUDORZ
SiN Film WHPSHUDWXUH 3(&9' 6L1 ILOPV ZHUH FRPSDUDEOH WR WKDW RI
KLJKWHPSHUDWXUH3(&9'6L1ILOPV)RUH[DPSOHWKHNc
ORZ 5) SRZHU ƕ& ILOP KDG D .F RI 03D¥P
Substrate VLPLODUWRWKH&KLJK5)SRZHUILOPRIWKHVDPHWKLFNQHVV
ZLWKD.FRI03D¥P
,Q JHQHUDO IUDFWXUH WRXJKQHVV LQFUHDVHG ZLWK LQFUHDVLQJ
5)SRZHUDQGLWYDULHGOLQHDUO\ZLWKLQFUHDVLQJWHPSHUDWXUHV
+RZHYHU IRU KLJK 5) SRZHU FRQGLWLRQV WKH IUDFWXUH
WRXJKQHVV ZDV RQO\ VHHQ WR FKDQJH YHU\ VOLJKWO\ IRU ERWK N
DQGNILOPVDPD[LPXPFKDQJHRIDERXWDVFRPSDUHG
WR WKDW DW ORZ 5) SRZHU D PD[LPXP FKDQJH RI 7KLV
VKRZHG WKDW WKH HIIHFW RI SURFHVVLQJ WHPSHUDWXUH ZDV QR
Platinum ORQJHU WKH PDMRU LQIOXHQFLQJ IDFWRU LQ WKH IUDFWXUH WRXJKQHVV
RIWKHILOPVDWKLJK5)SRZHUV
Coupon Surface )UDFWXUH WRXJKQHVV ZDV DOVR QRWLFHG WR JHQHUDOO\ LQFUHDVH
ZLWK LQFUHDVLQJ GHSRVLWLRQ WHPSHUDWXUH +RZHYHU WKH Nc
SiN Film KLJKSRZHUILOPVGLGQRWVKRZVXFKDWUHQG,WZDVOLNHO\GXH
WRWKHODUJHHUURUIRU&RXSRQ¶VUHVXOWVZKLFKKDGDOLPLWHG
QXPEHU RI VXFFHVVIXO LQGHQWDWLRQV XSRQ WKDW UHVXOWHG
Substrate LQDQXQXVXDOO\ODUJHPHDQ.FYDOXH6OLJKWO\ORZHU.FYDOXHV
DUHH[SHFWHGIRUFRXSRQXSRQUHSHDWRIWKHH[SHULPHQW
0HDQFUDFNOHQJWKV FLQWKH LQGHQWDWLRQV7DEOH ZHUH
DOO VKRZQ WR EH DERXW WR JUHDWHU WKDQ WKH ILOP
WKLFNQHVV 7KLV VXSSRUWV WKH DGRSWLRQ RI WKH FKDQQHO FUDFN
PRUSKRORJ\ PRGHO DV FRPSDUHG WR D KDOISHQQ\ UDGLDO RU
3DOPTYLVW FUDFN PRGHO DV WKH FUDFN OHQJWKV LQ WKH ODWWHU WZR
KDYHWREHOHVVWKDQWKHWKLFNQHVVRIWKHILOPLQRUGHUWRIRUP
KHPLVSKHULFDOUHJLRQVLQWKHILOP
),% UHVXOWV RI VRPH LQGHQWDWLRQV VKRZHG VOLJKW
GHODPLQDWLRQ HIIHFWV DV VHHQ LQ )LJXUH &RPSDUDWLYHO\
)LJXUH ZDV DQ H[DPSOH RI DQ LQGHQWDWLRQ WKDW FDXVHG QR
GHODPLQDWLRQ 7KH LQGHQWDWLRQV WKDW VKRZHG GHODPLQDWLRQ LQ
WKHFURVVVHFWLRQZHUHQRWVLJQLILFDQWHQRXJKWRFDXVH YLVLEOH
GHODPLQDWLRQ RQ WKH FRXSRQ VXUIDFH ,I WKH\ GLG WKH UHVXOWV