You are on page 1of 28
COSMETIC SPECIFICATIONS OF INJECTION MOLDED PARTS << Specifications for Molders and their customers 1994 Edition UNIFORM VIEWING CONDITIONS AND ACCEPTANCE CRITERIA KEys To COSMETIC INSPECTION OF PLASTIC MOLDED PARTS GLOSSARY OF TERMS FOR TYPICAL COSMETIC DEFECTS ‘Sponsored by the Molders Division of The Society of the Plastics Industry, Inc. The Society of the Plastics Industry Cosmetic Specifications of Injection Molded Parts This specification has been prepared by the Molders Division of The Society of the Plastics Industry, Inc. as a service to its members and their customers. The specification provides recommendations only. It is up to the molder and customer to determine particular contractual arrangements © 1994 The Society of the Plastics Industry, Inc. Acknowledgement ‘The SPI Molders Division is indebted to Carl Kem, Director of Quality, BACE Manufacturing, Inc., for his dedication to the development of this guide as its principal author and layout- designer. The division also wishes to thank Mike Nogele, CEO, BACE Manufacturing, Ine. (and ‘Molders Division Director-at-Large) for BACE’s generosity in providing the contents of the original draft. We also acknowledge Mr. Nogele's leadership towards achieving the published document. Questions or comments should be directed to: Molders Division ‘The Society of the Plastics Industry, Inc. 1275 K Street, NW Suite 400 Washintgion, DC 20005 Phone: (202) 371-5200 Fax: (202) 371-1022 ‘Version A Date of Issue: March , 1994 The Society of the Plastics Industry Cosmetic Specifications of Injection Molded Parts Table of Contents page I. Defect Definitions 2 I. Surface Identification and Classification of Surface Finish 8 IIL. Standard Viewing Condition 9 IV. Color Matching 10 V. Gloss 10 VI. Surface Finish and Texture Matching u ‘VIL. Adhesion u Cosmetic Quality Summary Sheets 12 Appendix 17 Version A © 1994 The Society of the Plastics Industry, Inc. The Society of the Plastics Industry Cosmetic Specifications of Injection Molded Parts TITLE: Cosmetic Specification of Injection Molded Parts PURPOSE ‘The purpose of this standard is to provide quantitative definitions, and recommended methods of inspection and measurement of the cosmetic quality attributes in the absence of customer provided specifications. ‘The definitions, descriptions and classifications contained in the specification are based on typical terms used in the injection molding process and, where applicable, also relate to post molding activities. SCOPE This specification addresses the cosmetic quality of molded plastic parts and related post molding activities. Page 1 Version A O The Society of the Plastics Industry Cosmetic Specifications of Injection Molded Parts I DEFECT DEFINITIONS BLEEDING (paint or decoration) Evidence of one color overlaping or altering another color (painting). Speading of pigment beyond the intended boudries (silk screen, printing), BLUSH Discoloration or change in gloss. Generally occurring at gate locations or abrupt, changes in wall thickness. BROKEN General damage. For example bent and/or broken tabs or ribs. BUBBLES Void pockets, typically seen only in transparent parts, May appear as a bulge or protrusion in an opaque part. BURNS Brown marks or streaks. (Also see gas marks.) COLD SLUG First material to enter mold during injection. Solid or semi-solid, this material leaves a distinct border with adjacent melted material similar in appearence to. weldlines. Page 2 © 1994 The Society of the Plastics Industry, Inc. Version A The Society of the Plastics Industry Cosmetic Specifications of Injection Molded Parts CONTAMINATION Large areas of discoloration from foreign matter or foreign material embedded in the surface of a part. CRACKING Stress induced splitting or fissures causing separation of material CRAZING Miltiple tiny cracks due to stress exerted on the part. DELAMINATION Separation (peeling) of layers of plastic DISCOLORATION Any change from the original color standard. Unintended, inconsistent color. DRAG MARKS. Clusters of scratches from plastic dragging against mold details when a partis ejected from a mold EILL-INS (print or silk screen) ‘An excessive use of ink that alters the form of screened or printed feature. Placement of ink where no ink should be. Page 3 © 1994 The Society of the Plastics Industry, Inc. Version A The Society of the Plastics Industry Cosmetic Specifications of Injection Molded Parts ELASH Excess plastic at parting line or mating surface of the mold. Normally very thin and flat protrusion of plastic along an edge of a part. Can also appear as a very thin string or thread of plastic away from the edge of a part (string flash). Often found at vents, knock outs and other shut-off areas. FLOW MARKS (paint or silk screen) Waviness of edge or excessive linear junction between two surfaces of ink or paint, GAS MARKS Dark discolored streaks caused by incomplete venting of gases generated during the molding cycle. UGE ‘Surface imperfection due to abrasion that removes small amounts of material. ‘Depth is measurable. GREASE Any type of machine lubrication on the surface of a part. HAZE Cloudiness on an otherwise transparent part. Page 4 © 1994 The Society of the Plastics Industry, Inc. Version A The Society of the Plastics Industry Cosmetic Specifications of Injection Molded Parts INSERT PROBLEMS (Not a true "cosmetic" defect. More functional than cosmetic) Errors related to the installation of inserts into plastic parts. Inserts can be set too high or too low in a socket or boss. They can also be damaged or misaligned and may even be missing. JETTING See splay. LINT (paint) ‘Any unintended foreign substance in the coating or on the surface. MARBLING Colored streaks caused by incomplete mixing of 2 different colored plastics. Also referred to as streaking NICKS: Like gouges but of short length. Cause by impact rather than abrasion, NON-ADHESION (painted or decorated)) Lack of adequate sticking of paint, print or any coating to the plastic surface. ORANGE PEEL Rippled or mottled appearance view able as concentric lines. Caused by under- pressurizing. Orange peel is often the first sign of possible sink or shorting. Page 5 © 1994 The Society of the Plastics Industry, Inc. Version A The Society of the Plastics Industry Cosmetic Specifications of Injection Molded Parts PIN PUSH Protrusion or distortion caused by an ejector pin pushing into part more than normal. The protrusion is most evident on the surface opposite the ejector pin. PITTING Crater-like imperfections on the surface of the part, PULLING Part distortion caused from plastic catching in the mold when the part is ejected. RUNS (painting or printing) Dripping or sagging of paint or ink. Movement of ink beyond intended surfaces. Usually caused by too much or too thick paint or ink. SCRATCH Surface imperfection due to abrasion that removes small amounts of material Depth is not measurable. Differs from scratch in mold which leaves a consistent mark, ‘SHINE Glossy or shiny areas on textured surface. Usually caused by a dirty or worn ‘mold. Can also be caused by lack of sufficient pressure to properly replicate texture in the mold. Page 6 © 1994 The Society of the Plastics Industry, Inc. Version A. The Society of the Plastics Industry Cosmetic Specifications of Injection Molded Parts SHORTS (Short shot, non-fill) Missing plastic due to incomplete filing of the mold cavity. Parts are not completely formed. Can usually be identified by smooth, shiny and rounded surfaces. SINK ‘Surface depression caused by non uniform material solidification and shrinkage. Most often noted at interface between differing wall thicknesses. SMEARING (paint or ink) Similar to bleeding. Excess ink or paint in areas that should be free of ink or paint. ‘Smearing is due to rubbing of surface before adequately dried. SPECKS Small discolored points of matter embedded in the surface. Typically black, caused by material contamination or material degradation. SPLAY Off colored streaking. Usually appears silver-like. Splay is caused by moisture in the material or thermal degradation of the resin during processing. A similar look ‘can be caused by cold material skipping across the surface during a fast fill. This is commonly called "jetting" WELDLINES Witness line where 2 or more fronts of molten plastic converge. Also called kaitlines or flowlines, Page 7 © 1994 The Society of the Plastics Industry, Inc. ‘Version A The Society of the Plastics Industry Cosmetic Specifications of Injection Molded Parts I. SURFACE IDENTIFICATION AND CLASSIFICATION OF SURFACE FINISH A. SURFACE FINISH GRADE 1 - ‘+ Highly polished: (e.g. SPI - B1 or lower). ‘+ Clear transparent. + Fluid contact - (primarily applies to medical parts) GRADE 2- + Low grade polish, non-textured: (e.g. SPI - B2 or higher.) + Textured. + Clear translucent. GRADE 3 - + Painted parts GRADE 4- «Ink stamped, printed, silk screened + Other decorative processes. B. SURFACE IDENTIFICATION "AM surface - The top or front, most often viewed surface. Generally the front edge and sides of a part. Not viewed as often as an "A" surface but easily seen by user. "C" surface - Most often, the back and bottom surface. “"D" surface - internal surfaces. Normally D surfaces are not inspected for cosmetic attributes. Where, necessary, D surface inspection will be specified as an exception Page 8 © 1994 The Society of the Plastics Industry, Inc. ‘Version A The Society of the Plastics Industry Cosmetic Specifications of Injection Molded Parts Ill. STANDARD VIEWING CONDITION A. LIGHTING INTENSITY All quality decisions of cosmetic acceptability will be made under normal lighting conditions (80-120 footcandles) in white fluorescent light. B. VIEWING ANGLE All viewing will take place with direct overhead lighting. Viewing angle is dependent on surface classification In every case, parts will be held such that the light is NOT REFLECTED directly to the viewer. A" surface - Hold part 30° from the horizontal plane. Part is in direct line with your eyes. ROTATE part 30° to the right and to the left about the vertical "BY surface - Hold part 90° from the horizontal plane. Part is in direct line with your eyes, DO NOT rotate the part. "C* surface - Hold part 90° from the horizontal plane. Part is NOT in direct line with your eyes. Part is held 45° below the plane of your eyes. DO NOT rotate the part. C. VIEWING DISTANCE "A" surface - 18 inches "B" surface - 24 inches C" surface - 30 inches Page 9 © 1994 The Society ofthe Plastics Industry, Inc. Version A The Society of the Plastics Industry Cosmetic Specifications of Injection Molded Parts III. STANDARD VIEWING CONDITION (continued) | D. INSPECTION INTERVAL (time) | Inspection interval is a function of surface area. “AN non-"A" SURFACE AREA Surfaces Surfaces . | <4in? = (2"x2") 2 sec. 1 see. | 4-16 in? (4"x 4") 4 sec. 2 sec. | 16-64 in? (8"x 8") 6 sec. 3 sec. 64-144 in? (12"x 12") 8 see. 4 sec >144in2 12" x 12") 10 sec. 5 sec. IV. COLOR MATCHING | Decisions regarding color matching are made by comparison to known standards using a spectrophotometer, color meter or suitable color matching light booth. Color standards and tolerances shall be provided by the customer. In the absence of a customer supplied color standard, standards shall be developed based upon the material manufacturer's color chip set and tolerances shall be set using a Delta E (AE) limit of 1.00, unless otherwise stated by the customer. V. GLOSS. Determination of gloss is to be made using a suitable glossmeter (e.g. BYK Gardener Glossgard® 60° glossmeter). When gloss cannot be measured by glossmeter, judgement shall be made by eye against gloss standards provided by or approved by the customer. All evaluations by eye shall be under standard viewing conditions a Page 10 © 1994 The Society ofthe Plastics Industry, Inc. Version A The Society of the Plastics Industry Cosmetic Specifications of Injection Molded Parts VI. SURFACE FINISH and TEXTURE MATCHING. Judgement as to the conformance of surface finish is to be made by comparing a part to an SPI Mold Finish Guide plaque. Comparison is by eye unless otherwise specified by the customer, Judgement as to the conformance of surface texture is to be made by comparing a part to a Mold-Tech texture plaque. Comparison is by eye unless otherwise specified by the customer. VII. ADHESION Adhesion requirements pertain to printed, painted or other decorative finishes applied to the surface of a plastic part. The applied finish must withstand a tape test, whereby a piece of pressure sensitive tape (Scotch Number 610 or equivalent adhesive strength) is applied across the finished surface, The tape is then removed by rapidly pulling the tape at a 90 degree angle to the part surface. The tape is examined for evidence of finish coat removal. There should be no evidence of finish coat on the tape Page 11 © 1994 The Society ofthe Plastics Industry, Inc. Version A The Society of the Plastics Industry Cosmetic Specifications of Injection Molded Parts COSMETIC QUALITY SUMMARY SHEETS The following four pages are summary sheets outlining the cosmetic requirements by prade. Page 12 © 1994 The Society ofthe Plastics Industry, Inc. Version A The Society of the Plastics Industry Cosmetic Specifications of Injection Molded Parts GRADE 1 (Highly polished, clear transparent, fluid contact) SURFACE A B c WELDLINES Limite fr BLUSH and WELDLINES ar etaliched in agreement with ectomer & BLUSH and held based upon iit samples SINK ‘None alowed. 003" max 10" max SPECKS & ACCEPT IF- Lesthanor equal estan or equal Les than rege BUBBLES {0 010", Nocloser to 0107 No closer 10.012". Noclser than ach ‘than inc ‘han inch ALLOWABLE 0107-025". o10"- 025°. 012"- 030" RANGE ‘Allow 1 per 16 int? ‘Allow 2 pr 16 ink? ‘Allow 4 pe 16 inc? weary (6x4) No close (rx) No closer ‘tan 2 ince than inches, RESECTIF- Greater than 025", Greate tan 025". Greater han.030" SCRATCHES ‘ACCEPTIF- 100% or less in length 150" oes in length, 300" or less in length. ‘Allow I per 16 inch? ‘Allow I per 16 inch ‘Allow 2 per 16 ch? area, ray (47 x4"), No closer than Tine REJECTIF- Greater than 100" Greater than 150" Greater than 300° ———— SPLAY BURNS GAS MARKS MARBLING ORANGE PEEL NON-UNIFORM TEXTURE, PITTING ‘CRACKING CRAZING DELAMINATION COLD SLUGS : None Allowed None Allowed ‘Refetoimit samples ornate excpions in Quality Pen. —_—_——— © 1994 The Society of the Plastics Industry, Inc. Page 13, ‘Version A The Society of the Plastics Industry Cosmetic Specifications of Injection Molded Parts GRADE 2 - (Low grade polish, textured, clear translucent) SURFACE A B c WELDLINES Limits or BLUSH and WELDLINES ae eb arene wth comer & BLUSH sod dbase pe it empes SINK one alowed 005 me O15 max SPECKS & ACCEPT IF- Less than or equal ‘Less than or equal ‘Less than or equal BUBBLES 10.0107 Node {0.010 Node 10.0151 Nadler ‘tan ich than Vic tan ch ALLOWABLE 910"- 020: o1or-030 o1s- ow RANGE Allow pe inc? ‘Aw 2 pr 1 int? ‘Alow 3 pe sink? ore Gina Nocoeer (ne Node than? ten {tania RERCTIF- Grate. 030 rete tan 030% retrain SCRATCHES ‘ACCEPTIF- 130" orlessin length 200" o es in length 300" ores in Length Allow 1 per 16 inch? ‘Allow I per 16 inch? Allow 3 per 16 inch? xan, (area (4x4) No loser than inch, REJECTIF- Greater than 150" Greater than 200" Greater than 300" SPLAY ne Allowed None Allowed Refit it samples BURNS . . ‘ornate exceptions in GAS MARKS . : ality Plan. MARBLING. . : ORANGE PEEL. : 2 DELAMINATION 0 COLD SLUGS . : Page 14 © 1994 The Society ofthe Plastics Industy, Inc Version A The Society of the Plastics Industry Cosmetic Specifications of Injection Molded Parts GRADE - (Painted / Finished parts) SURFACE, A B c pisssinisinsssss ss en ee EEE SPECKS, DISCOLORATION, & GLOSSINESS ACCEPTIF-—Lassthan or equal es than or egal Less thane equ 1.010" No doser 10.015" Nocoser wis, than och ‘than ach. ALLOWABLE 010"-.020" nso 015" -.050" RANGE ‘Allow 3 pe 1 nck? ‘Allow 4 pr 16 inc? ‘Allow 6 pr 16 ick? wey (ra Nocloser (area No closer ‘than 2 inches. than Hines REIECTIF-— Greser than 020" Greater han 040". Greater han 050°, eae SCRATCHES & LINT ACCEPTIF: 010" x 030" o ess (020 x. 050" or less, 020x500" ores ‘Allow 2 pee 16 inck® ‘Allow 4 pe 16 inch ‘Allow 4 per 16 inch (4r x4"). No closer than (4" x4") No closer th (4" x4"), No closer than Tinh, Tin, Tin, REJECTIF- Greaterthan 010"%.030" Greater than 020" x.050" Greater than 020°x 500", MARKS & RUNS ACCEPTIF- none. 020" x.050" or less .020"x 500" ores ‘Allow 2 per 16 inch? ‘Allow 4 per 16 inch? ("x4") Nocloserthan (4x4). No closer than inch Vine REJECTIF- any found Greater than 020" x.050" Greater than 020 x 500" NON-ADHESION OR NON-UNIFORM COVERAGE ACCEPTIF- none. 125% or less 250" ores. ‘Allow 2 pe 16 inch Allow 4 pe 16 inch? Gtx4| Nocloserthan (4°14), No closer than inch inc, REJECTIF- any found Greater than 125" Greater than 250" Page 15 © 1994 The Society of the Plastics Industry, Inc. Version A The Society of the Plastics Industry Cosmetic Specifications of Injection Molded Parts GRADE 4 - (Decorated Parts - stamped, printed, silk screened, in-mold,... ete.)) SURFACE EN B c SPECKS, VOIDS & FILLINGS ACCEPTIF-—Lessthanor equal Les than equal ‘Less than equal {0 010", Noclose {0 015". Nodes wns. ‘han Tach. than Line, ALLOWABLE 010"-.020" 015-030" 025°» 050", ‘RANGE Allow 2 per 16 inch Allow 3 per 16 inch? “Allow 5 per 16 (era) No coer, @rxa| Nocloser (rea) Nocloee ‘han 2 inches. than Tach, than iach, REIECTIF- Greater than.020" (Greater than 030" restr than.050" FLOWMARKS & INCONSISTENCIES ACCEPTIF- none allowed 020" or ess. 00" or tess. ‘Allow 2 per surface ‘Allow 4 per surface [No loser than inch [No close than I inch REJECTIF- any found Greater than 020" Greater than 050", SMEARING, BLEEDING & HAZE ACCEPTIF- sone sllowed 020" ores 050" or less ‘Allow I per surace ‘Allow 2 per sure Noclose than inch —_‘Nocloserthan Unc, REJECTIF- any found reste than 020" reste than 50" Page 16 © 1994 The Society of the Plastics Industry, In. Version A The Society of the Plastics Industry Cosmetic Specifications of Injection Molded Parts APPENDIX ‘The following four pages are work sheets outlining the cosmetic requirements by grade and are intended to be used as work instructions at the job site. ‘Their use is optional and the sheets are provided merely as a tool in the implementation and integration of cosmetic evaluation during the manufacturing process (as opposed to after the process) The pages of the appendix may be photocopied Page 17 © 1994 The Society of the Plastics Industry, Inc Version A The Society of the Plastics Industry Cosmetic Specifications Cutomer: Part Name: Part Number: Authorized by: Light GRADE 1 (Highly polished, clear transparent, fluid contact) RRR nal SURFACE A B c aa <18" WELDLINES iit for BLUSH and WELDLINES ae elise in agreement wth csomer & BLUSH an el used up ii spas i SINK None allowed. 003° max 10" max. Saree a SPECKS & ACCEPT IF~ Lesthanorequal estan or ual Les than or esl BUBBLES 10.010" No done {0.0107 Noctoee 10.012" Nocoser than ick, than ch than inch ALLOWABLE 010"-.028, 010"-.025", 012". 030" RANGE Allow iper iin? ‘Allow 2 per 6 it? ‘Allow 4 per 1 ink? ore rx4) Noclorr (x4) Nocloer than 2 nce than ncn REJECTIF-— Gresterthan.025" rear than 025 ree than. 030" SCRATCHES ‘ACCEPT IF 100" ores in length 150" or ess in length 3100" ose ng ‘Allow 1 per 16 inch? ‘Allow 2 per 16 inc area (47x49) No closer than inch REJECT F- Greater than 100° Greater than 150° Greater than 300" ee SPLAY Noe Allowed Nine Allowed Refer toi smpes BURNS : . ot exons in ‘GAS MARKS : ay Plan MARBLING ° S ORANGE PEEL 2 ‘ 2 NON-UNIFORM TEXTURE * : : PITTING : : ‘CRACKING : 7 : CRAZING : : : DELAMINATION : ‘ : COLD SLUGS : : S — © 1994 The Society of the Plastics Industry, Inc. Version A The Society of the Plastics Industry Cosmetic Specifications Catomer | Part Name: Part Number: | Authorized by: | aR GRADE 2 - (Low grade polish, textured, clear translucent) al SURFACE A B c Lk at ee WELDLINES Lite for BLUSH and WELDLINES areal in azeonet with cme Daeg & BLUSH sd ed tated pen iit samples, rotate 8 SINK None lowe. 005" max ons me SE SPECKS & AccerT ir. Lesstanorequt estan or qu ethanol BUBBLES 10.010" Nodosr 10.010: No deer {0.015 No lor ‘tan ink ‘tan inh ‘han inh, ALLOWABLE 010-030. 210"- 030 ais" 040 RANGE ‘Allow prick? ‘low 2p iin? ‘ow’ pe Tin? one Gece Noster (ene Nocoer than 2 ches fia iak REIECTIF- Greater thn. 030, ret tan. ret than. 040, SCRATCHES ‘ACCEPT IF- 150" ores in eng. 200 resin ath 300" o less in ength. ‘Allow 1 pe 1 inc? ‘Allow | pertSinch® “Allow 3 per 16 ioc? ore Gat (44°), No closer than Vik RERCTIF- Grete reste than 3 SEE SPLAY None Allowed one Allowed Refer tint samples, BURNS . : ert exes in ‘GAS MARKS . 7 ‘Quality Plan, MARBLING : : : ORANGE PEEL 7 7 ” NON-UNIFORM TEXTURE. * . : PITTING : : ‘CRACKING - CRAZING : : DELAMINATION : . : COLD sLuGs : . ee © 1994 The Society of the Plastics Industry, Inc. Version A. The Society of the Plastics Industry Cosmetic Specifications Cutomer: Part Name: Part Number: Authorized by: . Light GRADE 3 - (Painted / Finished parts) SURFACE A B c | | SPECKS, DISCOLORATION, & GLOSSINESS | 4 | 30 deg ACCEFTIF- Lee than equa eset gn esha o equal rotate to-0)07 No cer te.01S" Node was ‘tan ink fhe nc e ALLOWABLE 010" -.020", L015" « 040". O15" - 050". RANGE Allow 2 per 16 inch? “Allow 4 per 16 inch? Allow 6 per 16 inch? « ore Gree No cer Gre Nolo than inches ‘han chen REIECTIF- — Greterthan 020% Grete tan 040 rear than. 050, c ——— rere ee SCRATCHES & LINT eg ACCEPTIF-010"x 030" octess 120" x.050" or kes 20°x, $00" ols ‘low 2 per 16 inch? ‘Allow 4 per 16 inh Allow 4 pr 16 inc? (@txa"|Nocloserthan (4°47) Nocloer than G4 No hn than Tint inch Tine REJECT IF Greater than O10"x.030" Greater than 20"x.050" Greater than 020’ 500", MARKS & RUNS. ACCEPTIF- none. 020" x.050" ores, .020'x $00" or es. ‘Allow 2 per 16 inch? Allow 4 pet 16 inch (4° 4") No closer than (4"x¢4") No closer than inch, inch REIECT IF any found Greater than 020" x.050" Greater than 020'x 5" NON-ADHESION OR NON-UNIFORM COVERAGE ACCEPTIF- none. 125" ores. 250" or less. ‘Allow 2 per 16 inch? Allow 4 per 16 inch? (4 x4") Nocloserthan ——_(4" x4) No loser than in ined, REJECTIF- any found Greater than 12: Greater than 250° a —— Eee © 1994 The Society of the Plastics Industry, Inc. Version A The Society of the Plastics Industry Cosmetic Specifications Cutomer: Part Name: Part Number: Authorized by: Light GRADE 3 - (Painted / Finished parts) RAR ae SURFACE A B c ie ‘SPECKS, DISCOLORATION, & GLOSSINESS "30 dea, ACCEPTIF Leshan orequl Les thane gual ‘es than equal rotate {0.010% Node to.015" Noceer tals ‘ha 1c than Vinh : ALLOWABLE 010"- 020 015". 040% O15". 050" RANGE, ‘Allow 2 per 16 inch? “Allow 4 pee 16 inet? Allow 6 per 16 inch? < ox (rx4") No ctor Gre) Noclomr ‘an 2 inches than nce, REJECTIF- Greate than 020" renter han 040" Gres tan.050. © SCRATCHES & LINT eg ACCEPTIF- 010" x.030" ores. 020" x. 050" oes. 020". 500" or tes. ‘Allow? per 16 inch? ‘Allow 4 per 16 inch ‘Allow pe 16 inch? (Area) Nocloserthan (4" x4"). Nocloserthan—_(4"x4") No loser than inch inch 1 inch REJECTIF- Greater than 010" x.030" Greater than 020"x.050" Greater than 20°x 500% MARKS & RUNS ACCEPTIF- none. £020" x.050" or les. 0207 x $00" or less ‘Allow 2 pe 16 inc? Allow 4 per 16 inch? ("x4"), Nocloserthan——(4"24") No closer than Tineh Tineh, REJECT IF- any found Greater than 020" x.050" Greater than 020" x.500*, NON-ADHESION OR NON-UNIFORM COVERAGE ACCEPTIF= none 125" oles 250" or less ‘Allow 2 per 16 inch? Allow 4 per 16 inch? (6x4) Nocloserthan (4° x4"). No closer than Vine Tiel, REJECTIF- any found Greater then 125" Greater than 250". © 1994 The Society of the Plastics Industry, Inc. Version A The Society of the Plastics Industry Cosmetic Specifications Cutomer: Part Name: Part Number: Authorized by: ana GRADE 4 - (Decorated Parts - stamped, printed, silk screened, in-molé,...etc.)) al SURFACE. A B c eit SRE SPECKS, VOIDS & FILLINGS | ns eee gee {o.010" No doe to.015" Nodes to02s" ‘tan inch than inch ALLOWABLE 010" 020 15-030 .ons"-.050" ‘RANGE ‘Allow 2 per 16 inch “Allow 3 per 16 inch? ‘Allow $ pee 16 inch? (erty No ciee Gre Neder Gra) Nodlome ‘han inches fant than in, c REJECTIF- Greater than 020". Greater than 030". Greater than 050". - 454°9 Fy QWMARKS & INCONSISTENCIES A ACCEPTTF- onesie ree 60" ort \ a || Allow 2 per surface Allow 4 per surface L Nodloserthan Linch, Noloser dan I inch. REC found reste than 02 Create than.050 I 'SMEARING, BLEEDING & HAZE ACCEPTIF- none allowed 020" or ess. 050" or les, ‘Allow 1 per surface ‘Allow 2 per surfice ‘No closer than 1 inch, [No closer than | inch RENECTIF- any found Greater than 020" Greater than 050". © 1994 The Society of the Plastics Industry, Inc ‘Version # OC ;

You might also like