Professional Documents
Culture Documents
Heat Resitant Steel Castings Materials PDF
Heat Resitant Steel Castings Materials PDF
Casting Materials
material delivery ASTM delivery technological properties (at room temperature) max. operation
JUNKER DIN-number specification A297 condition Rp 0.2 Rm A5 temperature
[N/mm²] [N/mm²] [%] [°C]
F1002S 1.4743 DIN EN 10295 - not annealed3) - - - 900
AF1101 1.4823 DIN EN 10295 HD not annealed3) ≥ 250 ≥ 550 ≥3 1100
UNS J93005
A1050 1.4825 DIN EN 10295 HF not annealed ≥ 230 ≥ 450 ≥ 15 900
UNS J92603
A1201 1.4848 DIN EN 10295 HK not annealed ≥ 220 ≥ 450 ≥8 1100
UNS J94224
A1224Nb 1.4855 DIN EN 10295 - not annealed ≥ 220 ≥ 450 ≥4 1050
A1234Nb 1.4859 DIN EN 10295 - not annealed ≥ 180 ≥ 440 ≥ 20 1050
A1237 1.4857 DIN EN 10295 HP not annealed ≥ 220 ≥ 440 ≥6 1100
UNS N08705
A1205 2.4879 DIN EN 10295 - not annealed ≥ 240 ≥ 440 ≥3 1150
Thermco 50 2.4778 DIN EN 10295 - not annealed ≥ 235 ≥ 490 ≥6 12001)
G-NiCr50Nb 2.4680 DIN EN 10295 - not annealed ≥ 230 ≥ 540 ≥8 10502)
G-NiCr15 2.4815 DIN EN 10295 - not annealed ≥ 200 ≥ 400 ≥8 1100
(9.4816)
) For cyclical heatings. the maximum temperature is 1100°C in air.
1
) This alloy will be applied up to a maximum operation temperature of 950°C under conditions with oil-ash-influence.
2