COLD SPLICING SYSTEM
FOR FABRIC CONVEYOR BELT
BANDO
PT. BANDO INDONESIA
JI, Gajah Tunggal, Desa Pasir Jaya,
Kecamatan Jati Uwung,
Kodya Tangerang
Telp. 021 - 5903938 & 5901311
Fax. 021 - 5903937
COLD SPLICING SYSTEM
1. 9 STEP COLD SPLICING
MENGGAMBAR SAMBUNGAN
BANDO
POTONG & KUPAS SUNPAT- Eco
PENGGERINDAAN
PEMBERSIHAN
PENGELEMAN
PENYAMBUNGAN
PENGEROLAN
FINISHING
CHECKING
2. MATERIAL COLD SPLICINGDASAR PEMILIHAN JENIS SAMBUNGAN
‘One ply strength < 250 Kg/em
Total belt strength < 1000 Ka/em
Thickness of cover rubber 0 ~ 6.5 mm
Cover rubber grade :
* General Use (Grade M, TIS-S, TIS-L)
* Oil Resistant ( OR - 210, OR ~ 220)
* Heat Resistant (HA - 510 )
(One ply strength > 250 Kg/em
‘Total belt strenath > 1250 Ka/em
Thickness of cover rubber > 6.5 mm
Cover rubber grade
* General Use (Grade M, 1IS-S, 1IS-L)
* Oil Resistant (OR - 210, OR - 220 )
= Heat Resistant (HR - 510, HR - 710)
* Fire Resistant ( FR - 300)
i
COLD SPLICING
HOT SPLICING
KETENTUAN YANG PERLU DIPERHATIKAN
KONSTRUKSI
Moulded edge ‘Top Caver Rubber
pene
[eee
1 Bottom cover Rubber
RuMUS SPLICING
(0.3 x B)+50+(S x (n-1))+25
keterrangan
L= Panjang Splicing (mm)
Lebar Bele (mm)
= Step Lengta (mm)
11 = jumah iy (lapisan canvas)
BELT DIMENSION
1. One ply strength
900 x EP 100 x 4P x 5.0 x 2.0 x 200
2. Overall belt strength
‘900 x NN 500 / 4 x 5.0 x 2.0 x 200
I bottom cover
Tebal top
umlah lapisan canvas
Kokuaten nominal belt
Jens fbrie (NN = Nylon, EP = Polyester)
shar betMEMBACA SPEC BELT
50x20: Ty Top rer dn oto cover
BSS Grade Cer al
pan
a
Kole z>F[e]s|[r][s]«]u
i oor | om | aon_| sour | sone | aone | anor | aon | ane | sono
fhe Fam [ana [ans | ane [ans | ane | amr | ans | an | a0
Ban | tan | Feo | Mar | ape | wis | sen | ot | ag | sep | om | Nov | Dee
7
SPLICING MATERIAL
MATERIAL COVER REMARKS
RUBBER
‘SUNPAT-ECO General Use | Belt strength (max) :
Hc - 510 Per Ply = 250 Kg/om
BUBBERICEMENTsso80 OR-210 Total Tebal = 1000Kg/em
1Kofkalena (0-71) OR -220 Tebal ibber = 6.51
ARETE tape - Tebal cover rubber = 6.5mm
75gr/Botel FR-300) | Pemakaian:
— 41Set=1M2
_— Cleaning Solvent
aaa
a ==
a
=SPLICING TOOLS
7 Ree
we
eye
=
Tar
Wwe |=
AN = |
A
F a
1. MENGGAMBAR SAMBUNGAN
Splicing Dimensions
» Bias (0.3 x B)
« Step Length (S )
« Titik / Garis Center
Tabel 1. Step Length
Fabric Strength | Step Length
(Kg/em ) {many
150
200
151-200 | 250
201 — 250 200
251-350 | 3502. POTONG & KUPAS
« Potong Sudut Bias
« Potong dan Kupas Cover
Rubber
2. POTONG & KUPAS
« Potong dan Kupas.
Canvas
e Potong dan Ratakan
Edge Gum. PENGGERINDAAN
» Gerinda & Keserkan Permukean.
Cover Rubber
4. PEMBERSIHAN
» Bersthkan permukaan
sambungan dengan sikat,
lanjutkan, dengan kain lap
yang dibasahi dengan
cleaning solvent5. PENGELEMAN
‘Slapkan 1 Set Lem Sumpat-ECO
(Cement + Hardnener).
Siapkan kaleng kosona sebagai
tempat untuk mengaduk Lem.
Oleskan Lem Pada permukaan
Sambungan, Kemudian Tunggu Sesaat.
40Menit .
Lanjutkan Pengeleman Kedua.
» Penyambungan Belt
Rekatkan kedua ujung
sambungan dengan
melepaskan plastiknya.
Note
Plastik dipakai untuk memudahkan meluruskan posis!
sambungan (Centering ).7. PENGEROLAN
Pengerolan
Lakukan pengerolan / pressing
padasatu arah keseluruh bagian
sambungasan.
» Pemotongan Sisa Ujung Cover
Rubber
» Rapikan Baglan Permukaan
Sambungan, Pinggir Belt
Dengan Mesin Buffing.
Bs9. CHECKING » Pemeriksaan Kelurusan dan
Penampilan Sambungan
TERIMA KASIH
BANDO
PT. BANDO INDONESIA
JI, Gajah Tunggal, Desa Pasir Jaya,
Kecamatan Jati Uwung,
Kodya Tangerang
Telp. 021 - 5903938 & 5901311
Fax. 021 - 5903937