omy Devanu:
DESCRIPTION
ISA UTAMA Fi
str Mezin &
‘SUMMARY OF INSPECTION
REPORT
Thepection/Recommendation Work Scope
JOURNAL BEARING
Finding
Exhibited corosion at overall surface
lower hat & axa of bearing
Recommendation :
|- Perform cleaning by chemical
|- Perform as received inspection
|- Apoly thinning material to base metal
|- Apaly new babbit layer with welding method
la per engineering standard
| Pecoum final inspection (Dimensional, UT & PT)
Found babbil condition heavy rubbing specially at
|- Remove ald babbit by heating torch or skin cut to base metal
|. Pecorm final machining process to target size as per drawing
oy Devanus:
RIANA iy
DIMENSIONAL INSPECTION REPORT
[OBNO- JOURNAL BEARING [MODEL TYPE, RENK TYPE ERNLG,
[CUSTOMER _: BADAKING [PN SIZE 14-160
IEQUIPMENT _: SONA TEST MS.380 [SN NA
JOEM RENK TYPE ERNLQ. INSP. DATE October 27-16, 202%
[nspectortevel SULARNATII_ |Report No. ‘OOTUT-MPKIDUFIXI2T
no] z 4 4 INO. 1 2
O° | 16000 | 100,02 160,05 1 JAa® 100 16002
0 rae[ 160.03 160.03
ce 159,99 160