You are on page 1of 1

Tensile Test report

Customer : Hanif Pre-load : 0,3 MPa


Test standard : DIN EN ISO 527-1 Speed, tensile modulus : 1 mm/min
Material : HDPE + Ampas Tebu 15% Test speed : 200 mm/min
Machine data : Zwick Z020 Grip to grip separation at the start position : 115,00 mm
Gage length, standard travel : 50 mm

Test results:
Force Et m m b b b h Travel Gage length, standard travel
Legend No. N MPa MPa % MPa % mm mm mm mm
1 528,82 282 13,5 25 13,5 25 10,06 3,88 19,25 50
2 529,24 291 13,7 28 13,7 28 10,04 3,85 34,47
3 534,73 288 13,8 26 13,8 26 10,06 3,84 24,48

Series graph:
20

15
Stress in MPa

10

0
0 50 100 150 200
Strain in %

Statistics:
Series Travel µ Force Et m m b b b h
n=3 mm N MPa MPa % MPa % mm mm
x 26,07 - 530,93 287 13,7 27 13,7 27 10,05 3,857
s 7,73 - 3,29 4,46 0,147 1,4 0,147 1,4 0,01155 0,02082
 [%] 29,65 - 0,62 1,55 1,07 5,38 1,07 5,38 0,11 0,54

2 Tensile HDPE + Ampas Tebu 15%.zs2 Page 1/1