eS as CHINLANSHING RUBBER VIETNAM INDUSTRIAL CO ., LTD
MATERIAL AND PRODUCT TEST RESULT ‘Check Confirm | Approval
Date : 17/11/2020 Report no:20201117005 P yy .
Material :2.3.1,2.3.3,4,5 Fomula: INNER:VO005 ,OUTER:CHCO12 |) ey, ht (2
/ }
Spec: $0212-4 Lot no: TEST { \ ey Sih
= t
ae Se
Testitem Test conditions | Specifications | Resutt | Judgment | Test method
Handness (Shore A) .
eae 7086 69 oK
original
properties [Tensile strength (MPa) 5
Cp Taree loess 5 min 109 oK — | astmpai2
ban
Elongation (%) ‘
gue aa 200 min 3142 ok — | astm D412
lHandness change (Shore A) . v
poem maa 28~0 10 oK
Ethanol
ae ea Tensile strength change (%) eee aa Pe
gasoline Le kéo tahy adi Fuel CE10, oer
resistance Elongation change (%) 23°C X 168h :
Khang xing o6 eee thay er -40 max 432 oK
jeén Ethanol [29 y
|Volume change (%) ‘
Thé tich thay adi oo mate UES or
Handness change (Shore A) Ee \
6 cimng thay adi 10416 ~ OF
Tensile strength change (%) v
seco tary i -15 max “10.1 oK
oil resistance IRM903 oil, ASTM pa7t
khang d2u |e crgation change (% taste x7on | as ‘| ox
186 gin dai thay di
|Volume change (%) 7 “7
7nd tich thay a6i ae a7 OK
lHandness change (Shore A) . 4g
126 cung thay adi et ug oe
[Sour gasoline
resistance {Tensile strength change (%) | Sour Gas #2 “aa0
Khang xang — |Lye kéo tahy ai ao'cxt4on | “0m $30 OK | ASTM DTI
|Sour gasoline
[Etongation change (%) .
150 gidn dai thay adi seu iat fo oe
IHandness change (Shore A) - Poin
86 cimng thay ai ome ca Oe
v ‘SAE J30-08
Heat aging Tensile strength change (%) | 4-0, . 4
Serie yer toe ey OW 450°C X 70h 48 max 28 ok | SECTION
Elongation change (%) .
150 gidn dai thay aéi Badd ee OKPetmanent compresion set (%) 5 y ASTM D395
Thir a6 bién dang 180°C X70n | 40 max oo ok | METHOD B
IL OUTER MATERIAL Vat ligu lop ngoai
Test item Test conditions | Specifications | Result | Judgment | Test method
Handness (Shore A) — ara cr
Original Be cang
properties —_[ Tensile strength (MPa) .
pac tinh co |e kéo 8 min 10 ox — | ASTM D412
ban
Elongation (%) 7
po arin de 200 min 200.4 ASTM D412
Handness change (Shore A) - =
126 ciang thay doi eee 7 a
Tensile strength change (%) +
oil resistance |Lyc kéo tahy di IRM903 oil, 20 mAX ee OK per]
Khang dau | Elongation change (%) 128°C X 70h qomax me oe
186 gin dai thay adi
Volume change (%) a 7
Thé tich thay ai seastee me ox
Handness change (Shore A) - v
186 cimng thay doi oui “4 on Ae J20-08
Heat aging [Tensile strength change (%) | 460, y SECTION
és hee |Lnoneo tanya 126°C X70h | -25max 0.0 ox om
[Elongation change (%) 7 7
D6 gidn dai thay ai ann fous a
Permanent compresion set (%) 5 . ‘ASTM D395
Thir do bién dang 128° X70n | 60-max 524 °K | METHOD B
Ill, HOSE PROPERTIES Thu nghigm san pham
Test tem Test conditions | Specifications | Result | Judgment | Test method
PTESTERTWI
Fuel CE10 for SAE J30-08
ee 48h X 23°C, PASS PASS oK SECTION
ee followed by 5h X| 65
20°C.
RE TIE
lOzone resistance 40°C X 70h X
og none Pageeal O Rating PASS oK ona
Burst resistance (Mpa) , v
Ap lve phd nly 0.4 min 1.34 ok — | ASTM D380
[Outer diameter change (2%) 4 :
Shay oi curong kinh ng! 150 KPaX5min| 0~ +15 2.31 oK
rau PreSSUTE OD change (Ey 7 AE JO0-0B ]
Thay d6i dung kinh ngoai khi hit chan 81kPaXxt6s | -20max 0.44 oK ‘SECTION
khong 64
JAdhesion between layers (Nimm) Ee
Luc bém dinh céc lop 0.4mmis 08 min pass ¥| OK sory
Total extractables (g/m?) v
Téng chat chiét xudt 2.5 max cau OK | sae 30-08
Extractables [76g ne
Frohuét wary exracabes (ai) 0.4 max o27 “| 0K 6.17
Sap chiét xudt
[Comment
Judge No
Thoi gian luu 20 nm QRO24-01