Environmentally Friendly Management

▶ Zinc strike plating process -1


1. Zn Die Cast pretreatment suggestion

Soak clean Electro clean Alkaline dip


Acid dip
(Reduction)

2. Aluminum pretreatment suggestion

Soak clean Etch Desmut

2nd zincate Cyanide cu strike


1st zincate Zincate strip

Electroless nickel

KOREA HOSUNG S/T CO., LTD.


Environmentally Friendly Management

• Zinc Die Cast Process


• Alkaline clean – Ultra 1012, 40 ~ 50℃ , 30sec ~ 2 min
• Rinse
• Alkaline Electro clean – Ultra 1012, 50 ~ 75℃, 0.5 ~ 1 ASD
Anodic, 30sec
• Rinse (X2)
• Acid dip – H2SO4 12ml/l, ACT KT 5~10g/l, 10~15sec.
• Rinse (X2)
• Reduction – NaCN 15g/l, Stripper F 50g/l, 35℃, 10~ 20sec.
• Rinse (X2)
• Cyanide Cu strike – 50℃, 2 ~ 3 ASD, 5 ~ 10 min, with current
• Rinse (X2)
• Activation – Nicate-480, 20 ~ 35℃, 10 ~ 20sec.
• Rinse (X2)
• Electroless nickel

KOREA HOSUNG S/T CO., LTD.