HOT WORK TOOL STEEL

2714
STEEL GRADES:
DIN : 56NiCrMoV7 EN : 35 CrMo 8 AISI : 6F3

CHEMICAL COMPOSITION: C 0.56 Cr 1.1 Mo 0.5 Ni 1.7 V 0.1

STEEL PROPERTIES: Tough die steel with high resistance to tempering and full quenching and tempering. This grade is usually supplied in annealed condition or quenched and tempered to an installed hardness of 370-410 HB (round) or 355-400 HB (square, flat). PHYSICAL PROPERTIES: Coefficient of thermal expansion
10-6 m/(m.k) 20-100 12.2 20-200 13.0 20-300 13.3 20-400 13.7 20-500 14.2 20-600 oC 14.4

Thermal conductivity W/m.K)

20 36.0

350 38.0

700 oC 35.0

APPLICATIONS: Highly tough standard tool steel for medium and big sized forging dies, is usually delivered in hardened and tempered condition. Hot shear blades, extrusion rams, die holders, supporting tools.

HEAT TREATMENT:
Soft Annealing Stress Relieving Hardening Tempering Temperature 650 700 oC 600 650 oC 840 870 oC 860 890 oC 300 600 oC Time 2 5 hours 2 hours Group 2 For 20 mm 1h. min 2 hours 300 52 1790 400 49 1620 450 47 1530 500 46 1480 Cooling Furnace Furnace Oil Air Air

Tempering After quenching in oil Tempering After quenching in oil

C HRC N/mm2

100 57 2120

200 54 1910

550 43 1360

600 38 1200

650 34 1080

o C HRC N/mm2

100 55 1980

200 52 1790

300 50 1670

400 47 1530

500 45 1440

550 43 1360

600 40 1260

650 36 1140

700 32 1020

Special Info: Can be nitride, preheating to 200-300oC prior work is necessary.