You are on page 1of 1

STANDARD WELDING CONDITION

Austenitic Heat
Welding Welding Carbon 3.5%Ni Low Alloy
Dia.(mm) Stainless Inconel Hastelloy Nickel Resist. Remarks
Condition Process Steel Steel Steel
Steel Cast Steel
2.0
GTAW 70-200 70-200 70-200 50-200 100-200 60-220 50-200 80-150
2.4
Current
2.6 60-100 55-85 55-90 50-90 NA NA NA NA
(A)
SMAW 3.2 80-140 90-130 90-140 70-120 80-120 NA NA 80-120
4.0 110-190 130-180 140-190 100-150 120-150 NA NA 80-150
2.0
GTAW 9-15 9-15 9-15 9-15 10-20 10-20 10-20 10-16
2.4
Voltage
2.6 21-24 21-24 21-24 18-22 NA NA NA NA
(V)
SMAW 3.2 22-27 22-27 22-27 20-25 20-30 NA NA 20-30
4.0 24-29 24-29 24-29 22-27 20-30 NA NA 20-30
2.0
GTAW 5-15 5-15 5-15 5-15 5-15 5-15 5-15 8-15
Travel 2.4
Speed 2.6 5-12 5-12 5-12 5-20 NA NA NA NA
(cm/min) SMAW 3.2 5-12 5-12 5-12 5-20 7-15 NA NA 7-15
4.0 5-12 5-12 5-12 5-20 7-15 NA NA 7-15