Repair report inspection Date: 02/08/19

Non Conformity report N°. 5 Motor Bridges M1 and M2


HDG repairs Fulcrum Project.
Client. SPG Dry Cooling
Non conformity description from Client:

1. Drain holes with irregular edges, according to AWS D1.1 :2015 sec. 5.14.8.3. 
2. Drain holes crowded of zinc, according to AWS 5.16.1 D1.1 sec. 5.16.1 & 5.16.2. 
3. Some items with sharp edges and drills (see Technical Purchase Specification for Structural Steel 5.5). 
4. Evidence of black spots which means some of the areas are not galvanized. ASTM A‐123 2017. 
5. Galva surface is not smooth, uniform and/or continuous. ASTM A‐123/6.2, 2017. 
6. Inadequate cleaning of the structure. Weld finish is not smooth or uniform. Spatters as well as cleaning condition 
before galvanizing is not acceptable, according to AWS D.1 :2015 sec. 6.9. 
7. The bleeding rust in such holes must be sealed off with welding and touched‐up with galvanizing to avoid rust. 
 
Actions done to close each point: 
1. The holes were closing with welding same WPS used for steel structure manufacturing with satisfactory results. 

 
 
Sheet 1 of 6 
 
2. Defect solved with action made in point 1. 

 
 
 
 
 
 
 
 
 
 
 
 
 
 
Sheet 2 of 6 
 
3. These sharp edges were smoothening and restored its functionality. 

 
 
4. Cleaned and applied Cold galvanized. 

 
 
Sheet 3 of 6 
 
5. Also, in the ASTM‐23/17 indicates that if this texture or uniformity don’t affect the functionality of your pieces, the 
surface is acceptable: 

… 
 
6. Were cleaned and resolved. 
7. Done. 

 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
Sheet 4 of 6 
 
 
Attachments. 
Thickness of cold galvanizing coat in repairs. 

 
Sheet 5 of 6 
 