INTERNAL TEST RESULT

Concrete Admixture Properties Test


HB Speed Series ex Pendawa Lestari
Descriptions :
Product Name : HB Speed C, HB Speed 2, & HB Speed C3
Project : Complaint – Pendawa Lestari
Trialmix Date : March 13, 2020
Author : M.Zaini Gani

QC Test :
- HB Speed C ex Tanki SBB By Pass
Tested Item Specification Test Result

Aspect Turbid Yellowish liquid Turbid Yellowish liquid


Density (gr/ml) 1.045 – 1.065 1.062
Solid Content (%) 28 – 31 30.66
pH value 4-5 4.72
Additional Test
Correlation Test by IR Analysis Min. 0.90 0.9403
IR Analysis :

PT. Sika Indonesia


Jl. Raya Cibinong- Bekasi km. 20, Limusnunggal- Cileungsi, BOGOR 16820 - Indonesia
Tel. +62 21 8230025 / Fax +62 21 8230025
Website : idn.sika.co.id
e-mail: sikacare@id.sika.com
INTERNAL TEST RESULT
Concrete Admixture Properties Test
HB Speed Series ex Pendawa Lestari
- HB Speed 2 ex Tanki SBB By Pass
Tested Item Specification Test Result

Aspect Clear Yellowish liquid Yellowish liquid


Density (gr/ml) 1.07 – 1.09 1.076
Solid Content (%) 38 – 41 39.22
pH value 4-6 4.43
Additional Test
Correlation Test by IR Analysis Min. 0.90 0.9636

IR Analysis :

PT. Sika Indonesia


Jl. Raya Cibinong- Bekasi km. 20, Limusnunggal- Cileungsi, BOGOR 16820 - Indonesia
Tel. +62 21 8230025 / Fax +62 21 8230025
Website : idn.sika.co.id
e-mail: sikacare@id.sika.com
INTERNAL TEST RESULT
Concrete Admixture Properties Test
HB Speed Series ex Pendawa Lestari
- HB Speed C3
Tested Item Specification Test Result
Tangki SBB B 9951 BDF B 9952 BDF B 9231 PDC
by Pass
Aspect Yellowish Liquid Clear liquid Clear liquid Clear liquid Clear liquid
Density (gr/ml) 1.29 – 1.33 1.327 1.301 1.327 1.207
Solid Content (%) 39 – 44 42.66 40.97 43.73 29.06
pH value Min.6 7.19 7.24 7.18 7.52
Additional Test
Correlation Test by IR Min. 0.90 0.9843 0.9673 0.9703 0.873
Analysis

IR Analysis :

PT. Sika Indonesia


Jl. Raya Cibinong- Bekasi km. 20, Limusnunggal- Cileungsi, BOGOR 16820 - Indonesia
Tel. +62 21 8230025 / Fax +62 21 8230025
Website : idn.sika.co.id
e-mail: sikacare@id.sika.com
INTERNAL TEST RESULT
Concrete Admixture Properties Test
HB Speed Series ex Pendawa Lestari
Test On Mortar (Minislump) :
Trial No. 1 2 3 4 5
MIX PROPORTION
OPC 450 450 450 450 450
Silica Sand 621 621 621 621 621
Dust 69 69 69 69 69
Agg 10-20 1080 1080 1080 1080 1080
Water/ vol 3 liter 360 360 360 360 360
Admixture
Viscocrete Series 0.90% 0.90% 0.90% 0.90% 0.90%
Redos HB Speed
HB Speed C3 ex Sika 1.50%
HB Speed C3 ex Tangki SBB Bypass 1.50%
HB Speed C3 ex B9951 BDF 1.50%
HB Speed C3 ex B9952 BDF 1.50%
HB Speed C3 ex B9231 PDC 1.50%
RESULTS
Slump :
Initial 11 11 11 11 11
Setelah HB Speed C3 11.5/26 11.5/26 11.5/25 11/25 11.5/26
Initial Set. Time (hh:mm) 3:20 3:20 3:35 3:30 3:50
Compresive Strength (Mpa)
6 Hours 9.70 10.90 10.80 9.80 7.30
8 Hours 15.30 16.60 17.80 15.40 12.30
1 day 40.35 39.37 39.13 38.86 36.41

PT. Sika Indonesia


Jl. Raya Cibinong- Bekasi km. 20, Limusnunggal- Cileungsi, BOGOR 16820 - Indonesia
Tel. +62 21 8230025 / Fax +62 21 8230025
Website : idn.sika.co.id
e-mail: sikacare@id.sika.com
INTERNAL TEST RESULT
Concrete Admixture Properties Test
HB Speed Series ex Pendawa Lestari
Test On Mortar (Minislump) :
Trial No. 1 2 3 4
MIX PROPORTION
OPC 450 450 450 450
Silica Sand 621 621 621 621
Dust 69 69 69 69
Agg 10-20 1080 1080 1080 1080
Water/ vol 3 liter 455 455 410 410
Admixture
HB Speed C ex Retained Sample QC 0.90%
HB Speed C Tangki SBB Bypass 0.90%
HB Speed 2 ex Retained Sample QC 0.90%
HB Speed 2 ex SBB By Pass 0.90%
RESULTS
Slump :
Initial 11/23 11.5/24 11.5/24 11.5/25
15’ 10 10 11/22 11/23
30’ 7 7 9 9
Initial Set. Time (hh:mm) 4:20 4:15 4:30 4:40
Compresive Strength (Mpa)
1 day 19.47 18.88 21.63 22.70
3 days 54.05 55.11 55.25 52.68
7 days - - - -

Summary :
Dari hasil test properties diatas, HB Speed C, HB Speed 2 & HB Speed C3 (selain HB Speed C3 ex B9231
PDC) masih sesuai sesuai spesifikasi Standart QC. Untuk Sample HB Speed C3 ex B9231 PDC ada penurunan
performa dan ada indikasi terkontaminasi dengan material lain. (bisa dilihat perbedaan solid content dan
hasil pada test mortar / minislump).

PT. Sika Indonesia


Jl. Raya Cibinong- Bekasi km. 20, Limusnunggal- Cileungsi, BOGOR 16820 - Indonesia
Tel. +62 21 8230025 / Fax +62 21 8230025
Website : idn.sika.co.id
e-mail: sikacare@id.sika.com
INTERNAL TEST RESULT
Concrete Admixture Properties Test
HB Speed Series ex Pendawa Lestari
The information contained herein and any other advice are given in good faith based on Sika's current knowledge and experience of
the products when properly stored, handled and applied under normal conditions in accordance with Sika's recommendations. The
information only applies to the application(s) and product(s) expressly referred to herein. In case of changes in the parameters of the
application, such as changes in substrates etc., or in case of a different application, consult Sika's Technical Service prior to using Sika
products. The information contained herein does not relieve the user of the products from testing them for the intended application and
purpose. All orders are accepted subject to our current terms of sale and delivery. Users must always refer to the most recent issue of
the local Product Data Sheet for the product concerned, copies of which will be supplied on request.

PT. Sika Indonesia


Jl. Raya Cibinong- Bekasi km. 20, Limusnunggal- Cileungsi, BOGOR 16820 - Indonesia
Tel. +62 21 8230025 / Fax +62 21 8230025
Website : idn.sika.co.id
e-mail: sikacare@id.sika.com

You might also like