You are on page 1of 18
BRITISH STANDARD Cold rolled narrow steel strip for heat treatment — Technical delivery conditions — Part 4: Spring steels and other applications ‘The aropean Standard EN 1122-42000 the sts ofa BSEN 10132-4:2000 BS EN 10152-42000 Soest National foreword ‘Tis Bai Sani te ofl ngs agg version of BN 10242000. ‘ogee wth BSEN 101501, nouperseas BS STO Pas 2 and 36 ‘The UX parison i its preparation was xt to Tecnica Camatee IBES1 Whougttecs whic asthe apenas ~ ald capi usin he et, — presto tho reponsible Bogen como ay eng o the [teetton, or pops for ea, and ey Oe U recess tomes, — monitor ried inartionl and European development ae pease em inte Oe 4. ts organzatons represented on eae ca be tae on et itecooetary Cross roferences ‘The Bt Sandu wich leet xeon or Barmpean pb asons feted ons docanent ay be four in the Bt Stare Catalog de he ‘etn ened Tremor Savares Corespendence nex” oy ig the Tac ofthe BS! Sends echose Case Ath Stara dows nt purport toe all te necessary proviso race User nt Sands re espa fore oro opison, ‘Comptiace witha British Standard does wot of self confer Saimunity ‘rom legal obligations. Summary of pages ‘Ts document compesos ont cover an ine nt core, the EN ie pe, pages Tan ela coer a aback conte ‘The Bt cop nc splayed i th document nics when he dooanant so Amendments issued since publication And No ]Dae | Gonmente EUROPEAN STANDARD EN 10132-4 NORME EUROPEENNE. EUROPAISCHE NORM February 2000 1087714010, 7.14028; 7714080 Enalsh version Cold rolled narrow steel strip for heat treatment - Technical delivery conditions - Part 4: Spring steels and other applications eri. Sure mun arc Pee a ‘ous Uubeorggi ee eso one ‘srt rs “ren ona Eperber ant cone wee CENCELELES Maal Raga a odio or gia i oon ‘Srcacxray be stnedcnsppeton ste Gata Seater say cea manage eee SA TNL Tip Compan Stearate fic ves (pes Fach Gamera ay ath non may anon ete roepnsiyel Gv mrar soning asada Ged Saseuhaan te ce (Ce eprten enna nn ars me of ri Opn Ce ele ann Fd Fn Chay Ca, (eth tn oy Liners anon ene Po bon See Saran nrc agion 2 Duis eomordey Se posal ean: Contec ce Seat BIOS Sse ‘0c Ag tae ny mary ny me ad rane en oraae0€ Page Contents Page Foreword 3 1 Scope 4 2 Normative references 4 3 Terms and definitions 4 4 Classification and designation 4 41 Classification 4 42 Designation 4 5 Information to be supplied by the purchaser 4 6 Manufacturing process 5 7 Requirements 5 7.4 General 5 1.2 Method of delivery 5 73. Delivery condition 5 7.4 Chemical composition 5 15 Mechanical properties 5 TS Stucture 6 1.7 Surface fish 6 7.8 Dimensions and tolerances on dimensions and shape 6 8 Inspe 6 8 Sampling 7 10 Test methods 7 11 Labelling, packaging and protection 7 12 Rotests 7 Annex A (informative): Technical information on steels for springs cn ‘and other applications Annex B (Informative): List of corresponding former national designations 14 Pagea en 101200 Foreword ‘This European Standard hes been prepared by Techrical Commitee ECISSITC 23, ‘Steels for heat treatment, alloy steels and free-cuiting steels - Qualies and éimensions, the secretariat of which is held by DIN. ‘This European Standard shal be given the status ofa national standard, ether by publication ofan identical text or by endorsement, a the latest by August 2000, anc Confctng national standards shall ba withdrawn at the latest by August 2000, ‘According to the CENICENELEC Internal Regulations, the national standards ‘organizations ofthe fllowing countries are bound to implement this Furopean Standard: Austra, Belgium, Czech Republic, Denmark, Finland, France, Germany, Greece, Iceland, ireland, italy, Luxembourg, Netherlands, Norway, Portugal, Spain, ‘Sweden, Switzerland and the United Kingdom. ‘The European Standard EN 10132, Cold coled narrow steel stip for heat-treatment - Technical delivery condiions, is subdivided as follows: Part 1: General Part 2: Case hardening steels; Part 3: Steels for quenching and tempering: Part 4: Spring steals and other special apolication. EN I0132.42000 1 Scope 4.4 This part of EN 10132 applies to: = nonalley and alloy cold rolled narrow steel stip thicknesses upto 6 mm; = non-aliey and alloy cold roiled narrow steel strip in the quenched and tempered ‘condition in thicknesses between 0,30 mm and 3,00 mm {for springs and for other special plications. 41.2 This EN 10132-4is complemented by EN 10132-1 2Normative references ‘This European Standard incorporates by dated or undated reference, provisions from ‘ther publications. These normative references are cited atthe appropriate places In the text and the publicatons are listed hereafter. For dated references, subsequent ‘amendments to oF revisions of any f these pubications apply to this European ‘Standard only when incerporaiad in it by amendment ar revision. For undated references the latest adion of the publication refered to applies. EN 10020, Definition and classification of grades of took EN 10132-1, Cold rolled narrow steel strip for heat treatment - Technical delivery ‘conditions - Part 1: General EN ISO 6508-1, Metall materials - Rockwel hardness test «Part 1: Test method (scales A, B,C; D,E, F, GH, K,N, T) (ISO 6508-1:1998). 3 Terms and definitions For the purposes ofthis standard, the terms and definitions given in EN 10132-1 apply. 4 Classification and designation 41 Classification All steels covered by this European Standard are classifi according to EN 10020, ‘Stool grates C58S, C605, C678, C75S, CBS, C90S, C1005 and C1255 are non-alloy special steals, steel grades 48SI7, 58SI7, 51ChV’4, BOCV2, 75NIB, 125Cr2 and 10206 are alloy special steels 4.2 Designation See EN 101321 '5 Information to be supplied by the purchaser ‘See EN 10192-1 ate. SSE Pages eu 10152-42000 6 Manufacturing process See EN 107524 7 Requirements 7A General See EN 1019244 7.2 Method of delivery Seo EN 101324 7.3 Delivery condition Cold rotted narrow steel strip covered by EN 10132-4 shall be supplied inane of the {allowing delivery conditions: — annesled or annesled and skin passed (+A or #0}; cold roled (#0); ‘quenched and tempered (+07). NOTE, The delivery cancion - annealed fo achive spheroidized carbides (*AC) -may be ‘agreed. In such cases, Ems on spheroiizaen and mochercal properties may also be agreed ‘tths tims of enquiry and oder 7.4 Chemical composition 7.4.41 Cast analysis, ‘The chemical composition shall be in socordance wit the values specified in Table 1 {or the cast analysis, 7.4.2 Product analysis In cases where a product analysis is requested, the admissible deviations from the values speciid for the cast analysis are indicated in Table 2. 7.5 Mechanical properties 7.5.1 Tensile properties and hardness, ‘The mechanical properties ofthe strip shal be in accordance withthe values given in Table 3. For thicknesses outsie this range, mechanical properties shall be agreed between the customer and the supplier. NOTE 1 For those customers who specify Rockwell harness catar than Vickers hardness or tense strength, a tables given in A, showing Rockwell hardness values for information. Pape EN o92.4:2000 NOTE 2. The steals may be quenched ino or fothermaly haat asta, Fr information, the ‘minimum harénese values ghan In Table 2 show tha minimum values aftr quenching, vlthout tempering NOTE 3. For spring applications, te preferred hardness range (HV) fr stelsaccorcing to ‘Table Sin the quenched and tempered contin are given in Tabi A3 fo information, 7.5.2Bend test Requirements for the bend test for steels in the annealed condition (+A) maybe agreed a the time of enquiry and order. 7.6 Structure 7.64 Grain size See EN 10132+1 7.6.2 Non-metallic inclusions See EN 1013241 7.833 Decarburization For silicon aloyed steels, decarburzation shal not excoed 3 % of the material thickness per side, for non-slicon alloyed steels, decarburization shall not exceed 2 % ofthe ‘material thickness per side when measured ata cstance of 5 mm from the stip edge {800 also EN 0132-1), 7.7 Surface finish “The surface finish of cold rolled narrow steel strip shall be bright as produced by rotlng ‘and annealing in a contoled atmosphere. “The surface fishes of quenched and tempered cold rolled strip are as folows: —reylblue oxide nish: unpolished; —brigth tempered: unpolished: — polishes: obiained by ne grinding, abrasive brushing or other processes; —polished and coloured: blue or yellow colour obtained by xidization by heat treatment, 118 Dimensions and tolerances on dimensions and shape See EN 107324. 8 Inspection See EN 10132-1 9 Sampling See EN 101324 410 Tost mothods ‘Soo EN 101321 11 Labolting, packaging and protection See EN 101324 12 Retests Soe EN 101924 Page en 101200 woae sew vem (stsAteue yse0) ,suoneoidde jeroads soupo pue sBurds 104 sjaays so uonssodwioo jeaqwio4y - | o1geL onnze-zei01 3 pode Pages ev so1s242b00 ‘Table 2- Permissible deviations between the product analysis and the limiting values given in Table 1 for the cast analysis Gre | Poriaaienemomenien | Pama aia ‘soya ‘sty {eer Dtoer sau ot spate ai bebo Pogo 10 EN T01%2-42000 Table 3 - Mechanic propertis and hardness requirements*® ‘So spat tweens swetecnarmmontamn | cateisver | consis nes (cnt som [omme | par |e, Par fw | as fm] ne fae > e eoner yeh lak tt on nd tn ea a rp stnmneacemi<350.m Farts cee mca gti te “ecient tesco rae tse SOY p09 SON 00 Kee + ey amgterataransgpmaeagticvensovton nue tere so apo + ae O25 asnec Re Tel eg te Seno an eth mH Veer ae Paget en o1a2cbe00 Annex A (informative) echnical information on steels for springs and other applications Table A.1 - Reference values for Rockwell hardness for steels for springs ‘Soe esgnaton cane conten rane | runbor | stand (Aor anand ‘Dastnpaneestn) eat Re ess | se °° aeons ous | van * sess cms | sa 3% sass cass | ane a sas 655 eros | sare os sast657 crass | se a sass? ear | 1500 6 massa sos | 18006 % saswesas wove | case oe casas wove | sa ® sass rowe | 1860 @ sasos25 vaso | +2002 a 0s “ace | sae ow 207 Fecha hardness Habe aged whee of eng snd rr, * Forte supsed inte quenched and tangas conan, 2298 ot SRC cal any io haceases = 40H and avnge AHR at Seah fer hrenes > OR ts Rose hares (le HRC Recharges (cle) Page 12 EN Tots2.42000 ‘Table A2- Reference values forthe heat treatment and the minimum hardnest ‘values in the quenched condition ‘St csston ‘Astanizoa | Quensing | Menu hare’ ha quenched Smee en Chrelennbou leroere same rerbar ct we cms sai oo ot a oo ere est estos a © = os va 01980 ot a 7 cms tare 7s01az0 a a 7 as stat eso vate 2 0 mov, 12286 016079 ow © 70 sca 12012 e010 0 co 2 720 =e mess range up wn ase rnin vaues apy 050 mmo 3.00 Re Rac harass ease Ch, WV Vener hardrac. age 19 Table A.3- Guidance values for hardness (HV) for material in different thicknoss ranges in the quenched and tempered condition [Seat eesanion ces HV he qunced ad teed cnn vane | nner Spee tense m) | a0 <082|950<07so751.00|100 180| 150200) 200300 CRS [feos [assess 5] 1551505 eas 9-5 | asina7s| ais wa08 Ges [ten ltssoass|ssswsis| astsos [es oaes | asecte| stow aes Gers [ita lagsoses|ssswsts| estos [es vas | aseare| aisw aes Ems [tau [Sor |s00. 0] ots [aes oats | coat | ssw ass cess ieee [Sotelo ss |atowose | ease srs| cao ee | Stas soos izir —_|Sosteos| ses wavs |sos.50| caste cus| costs | ses toss letons sare [Sostoos| ats wavs | ens 58 | ast ses) ces sts | costs lets [itene [SSstoos| ere wavs | eos ee | casi ces| ces sts | aes tss esr [taza les sts assis | eoteets| cao ets | sides Sor fis lssiate| seston | aeieaes| aswers | sistoses Sieve fists oo 5i0| sone so0|seS oats | oie ate| ete ds Seve [tise Est re Sosesee| seb oes | soars | ase sos "exe, [reese Fo0%ee0| sono see| ees vets | eeato| ao aas Boe [dee Eastesre| soso sse| easton | coors | aes cor fozoe [er asin sre sess sss) sas 50s | ae ost | ae oe Soo, BEE Page 14 EN s0182.42000 Annex B {ioformative) List of corresponding former national designations Table B.1 - List of corresponding former designations Ser ‘Stel designation ‘Comparatia foes sel designation in ‘scorang to name | numer | Germany | France utes | Fintand | Sweden Kingdom rame_| number as Tazoa | cuss | 11z05 | csoRR —cSs0 eas tian | Geeo | riz | coor soo ers trast | Geer | 1251] Caork C370 Ss tras | Gers | tiie | Grane cso0 as trae | Gees | ties | a ra0 tier | cero | sare | Stoo ese5 Grass taza | SPT NIN) Grose asa vat | 2 | | Geer Ser Manes | ssa | 15000 | sean Sion | terse | soon | tase | ‘stows aon | taza || 1 “ : ren vase | >] 1 | pewion 2 ‘sce tao | “ 10266 voor | 2 =| rocreree = BSEN 10132-4:2000 Ba 9 Chews High Road eden waiat, BSI — British Standards Institution ‘Bis te indent atonal body repens or prepvirg British Sanda I resets Ue UK vw ow standart Buope ane ate tetana ve is [worsted by Royal Cte Revisions Bets tates we uplate by amenvvent or eson Uses of Beh Stats Sho ak sae tha typos heat ends eo us teens im of 5 ingrove the uly of ou pret and series. We Weald be gatas gan ncciracyOr ipat we ng ‘Both Standard woul! en fhe Secreta a he tecucd soranee ecpantie, ‘Beenie wich can bound he se rn cove THEO) 55 9, asa 66a. stor meee an vidal upg servic aed PLUS which ensues tit Sttsesbes surely eevee te ter of sands Buying standards rds al BS, emutonl and eg andes plletins should be ‘treed Caer Soros Te 0208806 000.0) 896 701. ‘n resjonse to andes or tational sda, 8s BS poy to ply he BS plea o ose that have teen pulsed as Bosh Sane nes ‘Servant Information on standards St provides wide rang of norman cx national, Buropean sinatra ‘Sis tough abs) ants Teal Hep o Export [tener information series te ln aah ee ders on te ‘roduc unsere Contact dw infarsson Cer Te 28671) Fas oa aa0 708, Subseeg member of Sar ep pt te with standards lopment ond ‘coe ssn dcourts on he purchase pee sures For ata These and oer bene cotet Merry hentai Te 2) S072 ‘acon ion Copyright ‘Germ nin Spb, a el opt, UK of th ternal standard ‘This es ot elas the fee wn he couse of pln he aa | necessary ea cha bos a a, pe oe dest ase ‘ets eo be wed fr ay ces pe an pee he ee ‘ten permission f BST masta. I permission i gai the terns mag inde rray pagers or eens geen Dla nae ca be obese fom be Copa Maras ‘car aoo 7,

You might also like