You are on page 1of 12

PROYEK PEMBANGUNAN JUNCTION TOL

TEBING TINGGI

MILLSHEET
COMPRESSION TEST RESULT
ASTM C - 39
COMPOSITION MIX:
Client : PT.Hutama Waskita KSO 1. CEMENT : 550 Kg/m3
Project : Junction Tol Tebing Tinggi 2. SAND : 762 Kg/m3
Location : Tebing Tinggi 3. WATER : 121 Kg/m3
: 3. SPLIT 1-2 : 859 Kg/m3
Class : CLAS. AA/50 Mpa 4. SPLIT 05-10 : 183 Kg/m3
Max Agg : 19 mm 6. RETARDER : 0.42 Ltr/m3
7.Superplastisizer : 5.09 Ltr/m3
Girder Code : G1 (Junction) Speciment Cylinder 15 x 30 cm
Date Production : 29 Juni 2020 Area Cyl . cm2
1 KN . KG
1Mpa 10.937 KG

Date Age Weight Density Force Cylinder


Remarks
No CODE (days) (kg) (gr/cm³) Pressure Strength Average
Casting Tested
(KN) Mpa Mpa (%)

1 G1 29-Jun-20 06-Jul-20 7 12.900 2.433 812.4 46.89 93.79


12.880 2.430 853.9 49.29 98.58
12.670 2.390 844.2 48.73 49.31 97.46
12.800 2.414 890.3 51.39 102.78
12.840 2.422 870.4 50.24 100.48

𝜎𝑐𝑚 41.09 98.62


S 20.19
𝜎𝑐𝑘 10.48

Dibuat oleh, Disaksikan oleh,


PT. Waskita Beton Precast PT. Hakaaston

(............................) (............................)
PROYEK PEMBANGUNAN JUNCTION TOL

TEBING TINGGI

MILLSHEET
COMPRESSION TEST RESULT
ASTM C - 39
COMPOSITION MIX:
Client : PT.Hutama Waskita KSO 1. CEMENT : 550 Kg/m3
Project : Junction Tol Tebing Tinggi 2. SAND : 762 Kg/m3
Location : Tebing Tinggi 3. WATER : 121 Kg/m3
: 3. SPLIT 1-2 : 859 Kg/m3
Class : CLAS. AA/50 Mpa 4. SPLIT 05-10 : 183 Kg/m3
Max Agg : 19 mm 6. RETARDER : 0.42 Ltr/m3
7.Superplastisizer : 5.09 Ltr/m3

Girder Code : G2 (Junction) Speciment Cylinder 15 x 30 cm


Date Production : 1 Juli 2020 Area Cyl . cm2
1 KN . KG
1Mpa 10.937 KG

Date Age Weight Density Force Cylinder


Remarks
No CODE (days) (kg) (gr/cm³) Pressure Strength Average
Casting Tested
(KN) Mpa Mpa (%)

1 G2 01-Jul-20 08-Jul-20 7 12.950 2.443 771.8 44.55 89.10


12.920 2.437 742.9 42.88 85.76
12.970 2.447 800.3 46.19 45.02 92.39
12.940 2.441 790.7 45.64 91.28
12.990 2.450 794.2 45.84 91.69

𝜎𝑐𝑚 37.52 90.04


S 18.83
𝜎𝑐𝑘 8.96

Dibuat oleh, Disaksikan oleh,


PT. Waskita Beton Precast PT. Hakaaston

(............................) (............................)
PROYEK PEMBANGUNAN JUNCTION TOL

TEBING TINGGI

MILLSHEET
COMPRESSION TEST RESULT
ASTM C - 39
COMPOSITION MIX:
Client : PT.Hutama Waskita KSO 1. CEMENT : 550 Kg/m3
Project : Junction Tol Tebing Tinggi 2. SAND : 762 Kg/m3
Location : Tebing Tinggi 3. WATER : 121 Kg/m3
: 3. SPLIT 1-2 : 859 Kg/m3
Class : CLAS. AA/50 Mpa 4. SPLIT 05-10 : 183 Kg/m3
Max Agg : 19 mm 6. RETARDER : 0.42 Ltr/m3
7.Superplastisizer : 5.09 Ltr/m3

Girder Code : G3 (Junction) Speciment Cylinder 15 x 30 cm


Date Production : 2 Juli 2020 Area Cyl . cm2
1 KN . KG
1Mpa 10.937 KG

Date Age Weight Density Force Cylinder


Remarks
No CODE (days) (kg) (gr/cm³) Pressure Strength Average
Casting Tested
(KN) Mpa Mpa (%)

1 G3 02-Jul-20 09-Jul-20 7 12.950 2.443 801.3 46.25 92.50


12.920 2.437 766.9 44.27 88.53
12.990 2.450 792.4 45.74 45.86 91.48
12.910 2.435 811.8 46.86 93.72
12.940 2.441 800.2 46.19 92.38

𝜎𝑐𝑚 45.78 91.72


S 5.53
𝜎𝑐𝑘 36.93

Dibuat oleh, Disaksikan oleh,


PT. Waskita Beton Precast PT. Hakaaston

(............................) (............................)
PROYEK PEMBANGUNAN JUNCTION TOL

TEBING TINGGI

MILLSHEET
COMPRESSION TEST RESULT
ASTM C - 39
COMPOSITION MIX:
Client : PT.Hutama Waskita KSO 1. CEMENT : 550 Kg/m3
Project : Junction Tol Tebing Tinggi 2. SAND : 762 Kg/m3
Location : Tebing Tinggi 3. WATER : 121 Kg/m3
: 3. SPLIT 1-2 : 859 Kg/m3
Class : CLAS. AA/50 Mpa 4. SPLIT 05-10 : 183 Kg/m3
Max Agg : 19 mm 6. RETARDER : 0.42 Ltr/m3
7.Superplastisizer : 5.09 Ltr/m3

Girder Code : G4 (Junction) Speciment Cylinder 15 x 30 cm


Date Production : 3 Juli 2020 Area Cyl . cm2
1 KN . KG
1Mpa 10.937 KG

Date Age Weight Density Force Cylinder


Remarks
No CODE (days) (kg) (gr/cm³) Pressure Strength Average
Casting Tested
(KN) Mpa Mpa (%)

1 G4 03-Jul-20 10-Jul-20 7 12.950 2.443 791.8 45.70 91.41


12.970 2.447 808.3 46.66 93.31
12.980 2.448 804.3 46.43 46.30 92.85
12.930 2.439 794.9 45.88 91.77
12.940 2.441 811.2 46.82 93.65

𝜎𝑐𝑚 38.58 92.60


S 19.10
𝜎𝑐𝑘 9.61

Dibuat oleh, Disaksikan oleh,


PT. Waskita Beton Precast PT. Hakaaston

(............................) (............................)
PROYEK PEMBANGUNAN JUNCTION TOL

TEBING TINGGI

MILLSHEET
COMPRESSION TEST RESULT
ASTM C - 39
COMPOSITION MIX:
Client : PT.Hutama Waskita KSO 1. CEMENT : 550 Kg/m3
Project : Junction Tol Tebing Tinggi 2. SAND : 762 Kg/m3
Location : Tebing Tinggi 3. WATER : 121 Kg/m3
: 3. SPLIT 1-2 : 859 Kg/m3
Class : CLAS. AA/50 Mpa 4. SPLIT 05-10 : 183 Kg/m3
Max Agg : 19 mm 6. RETARDER : 0.42 Ltr/m3
7.Superplastisizer : 5.09 Ltr/m3

Girder Code : G5 (Junction) Speciment Cylinder 15 x 30 cm


Date Production : 4 Juli 2020 Area Cyl . cm2
1 KN . KG
1Mpa 10.937 KG

Date Age Weight Density Force Cylinder


Remarks
No CODE (days) (kg) (gr/cm³) Pressure Strength Average
Casting Tested
(KN) Mpa Mpa (%)

1 G5 04-Jul-20 11-Jul-20 7 12.940 2.441 813.6 46.96 93.92


12.950 2.443 810.7 46.79 93.59
12.930 2.439 812.6 46.90 47.17 93.81
12.870 2.428 817.5 47.19 94.37
12.940 2.441 831.2 47.98 95.96

𝜎𝑐𝑚 46.96 94.33


S 6.78
𝜎𝑐𝑘 36.10

Disaksikan oleh,
Dibuat oleh, PT. Hakaaston
PT. Waskita Beton Precast

(............................)
(............................)
PROYEK PEMBANGUNAN JUNCTION TOL

TEBING TINGGI

MILLSHEET
COMPRESSION TEST RESULT
ASTM C - 39
COMPOSITION MIX:
Client : PT.Hutama Waskita KSO 1. CEMENT : 550 Kg/m3
Project : Junction Tol Tebing Tinggi 2. SAND : 762 Kg/m3
Location : Tebing Tinggi 3. WATER : 121 Kg/m3
: 3. SPLIT 1-2 : 859 Kg/m3
Class : CLAS. AA/50 Mpa 4. SPLIT 05-10 : 183 Kg/m3
Max Agg : 19 mm 6. RETARDER : 0.42 Ltr/m3
7.Superplastisizer : 5.09 Ltr/m3

Girder Code : G6 (Junction) Speciment Cylinder 15 x 30 cm


Date Production : 6 Juli 2020 Area Cyl . cm2
1 KN . KG
1Mpa 10.937 KG

Date Age Weight Density Force Cylinder


Remarks
No CODE (days) (kg) (gr/cm³) Pressure Strength Average
Casting Tested
(KN) Mpa Mpa (%)

1 G6 06-Jul-20 13-Jul-20 7 12.740 2.403 800.1 46.18 92.37


12.930 2.439 792.7 45.76 91.51
12.880 2.430 750.8 43.34 45.27 86.67
12.910 2.435 794.3 45.85 91.70
12.940 2.441 783.5 45.22 90.45

𝜎𝑐𝑚 0.00 90.54


S 0.00
𝜎𝑐𝑘 0.00

Disaksikan oleh,
Dibuat oleh, PT. Hakaaston
PT. Waskita Beton Precast

(............................)
(............................)
PROYEK PEMBANGUNAN JUNCTION TOL

TEBING TINGGI

MILLSHEET
COMPRESSION TEST RESULT
ASTM C - 39
COMPOSITION MIX:
Client : PT.Hutama Waskita KSO 1. CEMENT : 550 Kg/m3
Project : Junction Tol Tebing Tinggi 2. SAND : 762 Kg/m3
Location : Tebing Tinggi 3. WATER : 121 Kg/m3
: 3. SPLIT 1-2 : 859 Kg/m3
Class : CLAS. AA/50 Mpa 4. SPLIT 05-10 : 183 Kg/m3
Max Agg : 19 mm 6. RETARDER : 0.42 Ltr/m3
7.Superplastisizer : 5.09 Ltr/m3

Girder Code : G7 (Junction) Speciment Cylinder 15 x 30 cm


Date Production : 7 Juli 2020 Area Cyl . cm2
1 KN . KG
1Mpa 10.937 KG

Date Age Weight Density Force Cylinder


Remarks
No CODE (days) (kg) (gr/cm³) Pressure Strength Average
Casting Tested
(KN) Mpa Mpa (%)

1 G7 07-Jul-20 14-Jul-20 7 12.830 2.420 762.9 44.04 88.07


12.850 2.424 810.2 46.77 93.53
12.980 2.448 794.3 45.85 45.78 91.70
12.850 2.424 792.8 45.76 91.52
12.770 2.409 805.1 46.47 92.94

𝜎𝑐𝑚 0.00 91.55


S 0.00
𝜎𝑐𝑘 0.00

Disaksikan oleh,
Dibuat oleh, PT. Hakaaston
PT. Waskita Beton Precast

(............................)
(............................)
PROYEK PEMBANGUNAN JUNCTION TOL

TEBING TINGGI

MILLSHEET
COMPRESSION TEST RESULT
ASTM C - 39
COMPOSITION MIX:
Client : PT.Hutama Waskita KSO 1. CEMENT : 550 Kg/m3
Project : Junction Tol Tebing Tinggi 2. SAND : 762 Kg/m3
Location : Tebing Tinggi 3. WATER : 121 Kg/m3
: 3. SPLIT 1-2 : 859 Kg/m3
Class : CLAS. AA/50 Mpa 4. SPLIT 05-10 : 183 Kg/m3
Max Agg : 19 mm 6. RETARDER : 0.42 Ltr/m3
7.Superplastisizer : 5.09 Ltr/m3

Girder Code : G8 (Junction) Speciment Cylinder 15 x 30 cm


Date Production : 8 Juli 2020 Area Cyl . cm2
1 KN . KG
1Mpa 10.937 KG

Date Age Weight Density Force Cylinder


Remarks
No CODE (days) (kg) (gr/cm³) Pressure Strength Average
Casting Tested
(KN) Mpa Mpa (%)

1 G8 08-Jul-20 15-Jul-20 7 12.940 2.441 739.6 42.69 85.38


12.880 2.430 740.8 42.76 85.52
12.950 2.443 759.4 43.83 44.13 87.67
12.930 2.439 779.2 44.98 89.95
12.970 2.447 803.3 46.37 92.74

𝜎𝑐𝑚 0.00 88.25


S 0.00
𝜎𝑐𝑘 0.00

Disaksikan oleh,
Dibuat oleh, PT. Hakaaston
PT. Waskita Beton Precast

(............................)
(............................)
PROYEK PEMBANGUNAN JUNCTION TOL

TEBING TINGGI

MILLSHEET
COMPRESSION TEST RESULT
ASTM C - 39
COMPOSITION MIX:
Client : PT.Hutama Waskita KSO 1. CEMENT : 550 Kg/m3
Project : Junction Tol Tebing Tinggi 2. SAND : 762 Kg/m3
Location : Tebing Tinggi 3. WATER : 121 Kg/m3
: 3. SPLIT 1-2 : 859 Kg/m3
Class : CLAS. AA/50 Mpa 4. SPLIT 05-10 : 183 Kg/m3
Max Agg : 19 mm 6. RETARDER : 0.42 Ltr/m3
7.Superplastisizer : 5.09 Ltr/m3

Girder Code : G9 (Junction) Speciment Cylinder 15 x 30 cm


Date Production : 9 Juli 2020 Area Cyl . cm2
1 KN . KG
1Mpa 10.937 KG

Date Age Weight Density Force Cylinder


Remarks
No CODE (days) (kg) (gr/cm³) Pressure Strength Average
Casting Tested
(KN) Mpa Mpa (%)

1 G9 09-Jul-20 16-Jul-20 7 12.890 2.431 774.8 44.72 89.45


12.900 2.433 791.5 45.69 91.37
12.830 2.420 764.4 44.12 45.26 88.24
12.870 2.428 790.2 45.61 91.22
12.610 2.379 799.6 46.15 92.31

𝜎𝑐𝑚 0.00 90.52


S 0.00
𝜎𝑐𝑘 0.00

Disaksikan oleh,
Dibuat oleh, PT. Hakaaston
PT. Waskita Beton Precast

(............................)
(............................)
PROYEK PEMBANGUNAN JUNCTION TOL

TEBING TINGGI

MILLSHEET
COMPRESSION TEST RESULT
ASTM C - 39
COMPOSITION MIX:
Client : PT.Hutama Waskita KSO 1. CEMENT : 550 Kg/m3
Project : Junction Tol Tebing Tinggi 2. SAND : 762 Kg/m3
Location : Tebing Tinggi 3. WATER : 121 Kg/m3
: 3. SPLIT 1-2 : 859 Kg/m3
Class : CLAS. AA/50 Mpa 4. SPLIT 05-10 : 183 Kg/m3
Max Agg : 19 mm 6. RETARDER : 0.42 Ltr/m3
7.Superplastisizer : 5.09 Ltr/m3

Girder Code : G10 (Junction) Speciment Cylinder 15 x 30 cm


Date Production : 10 Juli 2020 Area Cyl . cm2
1 KN . KG
1Mpa 10.937 KG

Date Age Weight Density Force Cylinder


Remarks
No CODE (days) (kg) (gr/cm³) Pressure Strength Average
Casting Tested
(KN) Mpa Mpa (%)

1 G10 10-Jul-20 17-Jul-20 7 12.840 2.422 788.4 45.51 91.02


12.890 2.431 811.4 46.84 93.67
12.820 2.418 796.2 45.96 45.68 91.92
12.860 2.426 804.7 46.45 92.90
12.890 2.431 756.4 43.66 87.32

𝜎𝑐𝑚 0.00 91.36


S 0.00
𝜎𝑐𝑘 0.00

Disaksikan oleh,
Dibuat oleh, PT. Hakaaston
PT. Waskita Beton Precast

(............................)
(............................)
PROYEK PEMBANGUNAN JUNCTION TOL

TEBING TINGGI

MILLSHEET
COMPRESSION TEST RESULT
ASTM C - 39
COMPOSITION MIX:
Client : PT.Hutama Waskita KSO 1. CEMENT : 550 Kg/m3
Project : Junction Tol Tebing Tinggi 2. SAND : 762 Kg/m3
Location : Tebing Tinggi 3. WATER : 121 Kg/m3
: 3. SPLIT 1-2 : 859 Kg/m3
Class : CLAS. AA/50 Mpa 4. SPLIT 05-10 : 183 Kg/m3
Max Agg : 19 mm 6. RETARDER : 0.42 Ltr/m3
7.Superplastisizer : 5.09 Ltr/m3

Girder Code : G11 (Junction) Speciment Cylinder 15 x 30 cm


Date Production : 11 Juli 2020 Area Cyl . cm2
1 KN . KG
1Mpa 10.937 KG

Date Age Weight Density Force Cylinder


Remarks
No CODE (days) (kg) (gr/cm³) Pressure Strength Average
Casting Tested
(KN) Mpa Mpa (%)

1 G11 11-Jul-20 18-Jul-20 7 12.890 2.431 784.3 45.27 90.54


12.840 2.422 780.5 45.05 90.10
12.880 2.430 750.3 43.31 44.32 86.62
12.670 2.390 740.9 42.77 85.53
12.930 2.439 782.9 45.19 90.38

𝜎𝑐𝑚 0.00 88.64


S 0.00
𝜎𝑐𝑘 0.00

Disaksikan oleh,
Dibuat oleh, PT. Hakaaston
PT. Waskita Beton Precast

(............................)
(............................)
PROYEK PEMBANGUNAN JUNCTION TOL

TEBING TINGGI

MILLSHEET
COMPRESSION TEST RESULT
ASTM C - 39
COMPOSITION MIX:
Client : PT.Hutama Waskita KSO 1. CEMENT : 550 Kg/m3
Project : Junction Tol Tebing Tinggi 2. SAND : 762 Kg/m3
Location : Tebing Tinggi 3. WATER : 121 Kg/m3
: 3. SPLIT 1-2 : 859 Kg/m3
Class : CLAS. AA/50 Mpa 4. SPLIT 05-10 : 183 Kg/m3
Max Agg : 19 mm 6. RETARDER : 0.42 Ltr/m3
7.Superplastisizer : 5.09 Ltr/m3

Girder Code : G12 (Junction) Speciment Cylinder 15 x 30 cm


Date Production : 13 Juli 2020 Area Cyl . cm2
1 KN . KG
1Mpa 10.937 KG

Date Age Weight Density Force Cylinder


Remarks
No CODE (days) (kg) (gr/cm³) Pressure Strength Average
Casting Tested
(KN) Mpa Mpa (%)

1 G12 13-Jul-20 20-Jul-20 7 12.870 2.428 750.3 43.31 86.62


12.720 2.399 780.4 45.05 90.09
12.950 2.443 761.7 43.97 43.90 87.93
12.640 2.384 770.6 44.48 88.96
12.840 2.422 739.5 42.69 85.37

𝜎𝑐𝑚 0.00 87.79


S 0.00
𝜎𝑐𝑘 0.00