SPECIFICATIONS 

     
PRODUCT SPECIFICATIONS
(Structural Steel and Sheet Pile)

Mechanical Properties

Yield
Yield Point Elogation Impact
Ratio
Type of N/mm2 (min.) % (min.) J (Min.)
tensile % (max.)
Classifications
Product
Strength
Thickness Thickness Thickness Thickness
N/mm2
16 ≤ t ≤ t≤ 5<t t
t ≤ 16 t ≥ 12 t >12
16 5 ≤ 16 >16

Structural SM40
245 235 400-510 - 23 18 22 27A
Steel 0

SM490 325 315 490-610 - 22 17 21 27A

TIS 1227 SM520 365 355 520-640 - 19 15 19 27A


1996
SS400 245 235 400-510 - 21 17 21 -

SS490 285 275 490-610 - 19 15 19 -

SS540 400 390 540 min - 16 13 17 -

SS400 245 235 400-510 - 21 17 21 -


JIS G3101
SS490 285 275 490-610 - 19 15 19 -
1995
SS540 400 390 540 min - 16 13 17 -

SM400
245 235 400-510 - 23 18 22 -
A

SM400
245 235 400-510 - 23 18 22 27A
B

SM490
325 315 490-610 - 22 17 21 -
JIS G3106 A
1995
SM490
325 315 490-610 - 22 17 21 27A
B

SM490
365 355 490-610 - 19 15 19 -
YA

SM490
365 355 490-610 - 19 15 19 27A
YB

JIS G3136 SN400 A 235 235 400-510 - 17 17 21 -


1994
SN400 B 235-335G 235-355 400-510 80H 18 18 22 27A
SN490 B 235-445G 325-445 490-610 80H 17 17 21 27A

43A 275 265 430-580 - 20 20 20 -

43B 275 265 430-580 - 20 20 20 27B

BS 4360 43C 275 265 430-580 - 20 20 20 27A


1986
50A 355 345 490-640 - 18 18 18 -

50B 355 345 490-640 - 18 18 18 27B

50C 355 345 490-640 - 18 18 18 27A

EN 10025 S275JR 275 265 410-560 - 22 22 22 27B


1993
S355JR 355 345 490-630 - 22 22 22 27B

1997 A36 250 400-550 - 20 -

A572
1997 290 415 min - 20 -
Gr.42
ASTM
A572
1997 345 450 minE - 18 -
Gr.50

1998 A992 345-450 450 min 85D 18 -

St 33 185 175 290 - 16  

St 37-2 235 225 340-470 - 24 -

DIN 17100 St 44-2 275 265 470-610 - 20 -

St 50-2 295 285 470-610 - 18 -

St 52-3 355 345 490-630 - 20 -

  t < 11 11 ≤ t ≤ 40        

250 260 250 410 min - 22 -

250LO 260 250 410 min - 22 -

350 360 340 480 min - 20 -


AS/NZS
350LO 360 340 480 min - 20 -
3679.1
1996 11 ≤ t
  t<11 t > 17        
≤ 40

300 320 300 280 440 min - 22 -

300LO 320 300 280 440 min - 22 -

Sheet Pile JIS A5528 SY295 295 490 min - 17 -


1988,
TIS 1390-
SY390 390 540 min - 15 -
1996

Remark - Carbon Equivalent (%) = C+Mn/6 + Si/24 +Ni/40 +Cr/5 +Mo/4 +V/14 (JIS Standard)
  - Carbon Equivalent (%) = C+Mn/6 + (Cr +Mo+V)/5 + (Ni +Cu)/15 (AS,ASTM Standard)
  - Chemical Composition on sensitivity of welding crack =C + Si/30 +Mn/20 + Cu/20 + Ni/60 +
Cr/20 + Mo/15 + V/10 + 5B
  - Bend test on material grades SS400, SS490, SS540
  - Additional chemical composition controls for material under grade A992 are as follows:
  Ni (max) = 0.45 , Cr (max.) =0.35 , Mo(max) =0.15 and mn/S (min.) = 20
  * : Nitrogen control exclude.
  SM 400 is suitable for welded structure . / เกรด SM400 เป็นเกรดทีเ่ หมาะ
สำหร ับโตรงสร้างทีม
่ ก ื่ ม
ี ารเชอ
  - SS 400 is suitable for general structure. /เกรด SS400 เป็นเกรดทีเ่ หมาะสำหร ับ
โครงสร้างทวไป
่ั
SPECIFICATIONS      
PRODUCT SPECIFICATIONS
(Structural Steel and Sheet Pile)

Chemical Compositions (ladle analysis)

Sensitivit
Carbon y
Classifications C Si P S N Cu
Equivalen of
(max. (max. Mn (max. (max. Nb V (max. (min.
t welding
) ) ) ) ) )
% (max.) crack
% (max.)

SM 060-
0.20 0.35 0.035 0.035 - - - - - -
400 1.40

1.6
SM490 0.18 0.55 0.035 0.035 - - - - - -
max

TIS 1227 1.6


SM520 0.20 0.55 0.035 0.035 - - - - - -
1996 max

SS400 - - - 0.050 0.050 - - - - - -

SS490 - - - 0.050 0.050 - - - - - -

1.6
SS540 0.30 - 0.040 0.040 - - - - - -
max

SS400 - - - 0.050 0.050 - - - - - -

JIS G3101 SS490 - - - 0.050 0.050 - - - - - -


1995
1.6
SS540 0.30 - 0.040 0.040 - - - - - -
max

JIS G3106 2.5x


SM400
1995 0.23 - C 0.035 0.035 - - - - - -
A
min.

SM400 0.60-
0.20 0.35 0.035 0.035 - - - - - -
B 1.40

SM490 1.6
0.20 0.55 0.035 0.035 - - - - - -
A max

SM490 0.18 0.55 1.6 0.035 0.035 - - - - - -


B max
SM490 1.6
0.20 0.55 0.035 0.035 - - - - - -
YA max

SM490 1.6
0.20 0.55 0.035 0.035 - - - - - -
YB max

SN400
0.24 - - 0.050 0.050 - - - - - -
A

JIS G3136 SN400 0.60-


0.20 0.35 0.030 0.015 0.36 0.26 - - - -
1994 B 1.40

SN490 1.6
0.18 0.55 0.030 0.015 0.44 0.29 - - - -
B max

1.6
43A 0.25 0.50 0.050 0.050 - - - - - -
max

1.5
43B 0.21 0.50 0.050 0.050 - - - - - -
max

1.5
43C 0.18 0.50 0.050 0.050 - - - - - -
max

BS 4360 0.003 0.003


1.6
1986 50A 0.23 0.50 0.050 0.050 - - - - - -
max
0.100 0.100

0.003 0.003
1.50C
50B 0.2C 0.50 0.050 0.050 - - - - - -
max
0.100 0.100

0.003 0.003
1.50C
50C 0.2C 0.50 0.050 0.050 - - - - - -
max
0.100 0.100

S275J 1.5
0.21 - 0.045 0.045 - - - - 0.009* -
EN 10025 R max
1993
S355J 1.6
0.24 0.55 0.045 0.045 - - - - 0.009* -
R max

199
A36 0.26 0.40 - 0.040 0.050 - - - -    
7

199 A572 1.35F 0.01-


0.21 0.40 0.040 0.050 - - - - -
AST 7 Gr.42 max 0.015
M
199 A572 1.35F 0.01-
0.23 0.40 0.040 0.050 - - - - -
7 Gr.50 max 0.015

199 0.10- 0.50- 0.05 0.11 0.6ma


A992 0.23 0.035 0.045 0.45 - 0.012
7 0.40 1.50 max max x

DIN St 33 - - - - - - - - - - -
17100
St 37- 0.17 - - 0.050 0.050 - - - - 0.009* -
2

St 44-
0.21 - - 0.050 0.050 - - - - 0.009* -
2

St 50-
- - - 0.050 0.050 - - - - 0.009* -
2

St 52-
0.2 - - 0.040 0.040 - - - - - -
3

                         

250 0.25 0.40 - 0.040 0.040 0.43 - - - - -

1.5
250LO 0.20 0.40 0.040 0.040 0.42 - - - - -
AS/NZS max
3679.1
1.6
1996 350 0.22 0.50 0.040 0.040 0.45 - - - - -
max

1.6
350LO 0.22 0.50 0.040 0.040 0.45 - - - - -
max

                         

1.6
300 0.22 0.50 0.040 0.040 0.44 - - - - -
max
 
1.6
300LO 0.22 0.50 0.040 0.040 0.44 - - - - -
max

JIS A5528 SY295 - - - 0.040 0.040 - - - - - 0.25


1998
TIS 1390- SY390 - - - 0.040 0.040 - - - - - 0.25
1996

Remark A : Impact test on material grades SM400,SM490, SM520,SM400B,SM490YB, SN400B,SN490B,


43C and 50C with thickness > 12 mm. at 0 ํC
  B : Impact test on material grades 43B, 50B, S275JR with thickness > 12mm. at 20 ํC
  C : It is permissible to vary the carbon and manganese contents (ladle analysis) for grades 50B
and 50C on the basis of an increase of 0.06% manganese content for each decrease of
0.01% carbon or vice versa up to maximum manganese content of 1.60% and maximum
carbon of 0.22% for grades 50B and 50C.
  D :The yield radio (max.) for all thickness of materials under grades A992 is 85%
  E : For grades 50 steel of thickness 20mmand under , the tensile strength shall be a minimum of
485 N/mm2.
  F : A maximum of manganese of 1.50% is permissible , with an associated reduction of the
carbon maximum of 0.03%
  G :For the h section, when the t1 s 9mm or less, the upper limit of the yield point or proof stress
shall not be applied.
  H :For the H section , when the t1 is 9mm or less, the upper limit of the yield radio shall be 85%
     
  - Material under TIS compulsory standard are for domestic use only , while
materials under other standards are for exportation.
     
  SM 400 is suitable for welded structure . / เกรด SM400 เป็นเกรดทีเ่ หมาะ
สำหร ับโตรงสร้างทีม
่ ก ื่ ม
ี ารเชอ
  - SS 400 is suitable for general structure. /เกรด SS400 เป็นเกรดทีเ่ หมาะ
สำหร ับโครงสร้างทวไป
่ั

TOLERANCES      
TIS1227 : 1996      

TIS 1227-1996

(HOT ROLLED H - SECTIONS)

Dimension Tolerance Remark

H<380 ± 2.0  

Depth (H) 380≤ H<580 ± 3.0

≥ 580 ± 4.0

B<95 ± 2.0

Width (B) 95≤ B<190 ± 2.5

≥ 190 ± 3.0

Thickness t1<16 ± 0.7


(t1, t2 )
t1 16≤ t1<25 ± 1.0

25≤ t1<40 ± 1.5

t2 t2<16 ± 1.0

16≤ t2<25 ± 1.5

25≤t2<40 ± 1.7
+ 40
L ≤ 7 m.
0
Length (L)
40+(no. of meter of L-7) x 5
L > 7 m.
0

B≤ 150 ≤1.5  
H≤ 300
B> 150 ≤1.0% of B
Squareness (T)
B≤ 125 ≤1.5
H> 300
B> 125 ≤1.2% of B

H≤ 300 ≤0.15% of L
To be applied to bend such as
Bend
H> 300 ≤0.10% of L sweep and camber 

H≤ 300,B≤ 200 ± 2.5  


Eccentricity (S)
H> 300,B> 200 ± 3.5

H<400 2.0  

Concavity of web (W) 400≤H<600 2.5

H≥ 600 3.0

H≤ 187.5 ≤3.0 mm.  

Squareness of cut end B≤ 187.5 ≤3.0 mm.


(e)
H> 187.5 ≤1.6% of H

B> 187.5 ≤1.6% of B

t<10 ± 5% 1. The maximum thickness


shall apply.
2. These tolerances shall
apply in the purchase of a
Mass (kg/m.) single set of structural steel of
T≥ 10 ± 4% the same size and thickness
comprising not less than 10
pieces and a mass of not less
than 1,000 kg.