CLIENT: - GREAT EASTERN

PROJECT :-G+2 BUILDING AT SREE RAMPORE


DATE :- 11/9/2022
DESIGN STIPULATION :-
GRADE OF CONCRETE M30
CONDITION OF EXPOSER SEVERE
TYPE OF CONCRETE RCC
MAXIMUM SIZE OF AGGREGATE IN MM 20
MODE OF PLACEMENT PILE
SLUMP SPECIFIED 175+-25 mm
TEST DATA :-
CEMENT CONTENT IN KG 430
TYPE OF CEMENT PSC
BRAND OF CEMENT ACC
SPECIFIC GRAVITY OF CEMENT 2.9
SOURCE OF COARSE AGGREGATE PANCHAMI
SOURCE OF FINE AGGREGATE ILAMBAZAR / DAMODAR
GRADING ZONE OF FINE AGGREGATE ZONE II
COARSE AGGREGATE FRACTION -I 20 mm
COARSE AGGREGATE FRACTION -II 10 mm
BLENDING PROPORTION OF COARSE AGGREGATE AND FINE COARSE 59 %
AGGREGATE FINE 41 %
COARSE AGGREGATE % FRACTION-1: 20 MM : 55 %
FRACTION-2: 10 MM : 45 %
FINE AGGREGATE = 41 %
COARSE AGGREGATE IN TOTAL AGGREGATE % FRACTION-1: 20 MM 32.45 %
FRACTION-2: 10 MM 26.55 %
FINE AGGREGATE IN TOTAL AGGREGATE % 41 %
SPECIFIC GRAVITY OF COARSE AGGREGATE FRACTION-1: 20 MM 2.83
FRACTION-2: 10 MM 2.8
SPECIFIC GRAVITY OF FINE AGGREGATE 2.62
WATER ABSORPTION OF COARSE AGGREGATE % FRACTION-1: 20 MM 0.7 %
FRACTION-2: 10 MM 0.8 %
WATER ABSORPTION OF FINE AGGREGATE 1.6 %
MOISTURE CONTENT OF COARSE AGGREGATE FRACTION-1: 20 MM 0 %
FRACTION-2: 10 MM 0 %
MOISTURE CONTENT OF FINE AGGREGATE 0 %
CHEMICAL ADMIXTURE :-
DOSAGES OF CHEMICAL ADMIXTURE (% BY WEIGHT OF CEMENT) 0.9
NAME OF THE ADMIXTURE ACC MP-5410