You are on page 1of 1

THANBEE PRINT WORLD LTD.

PRINT DURABILITY TEST REPORT

Buyer Name: — VF-The North Face Received Date: — 27/01/2024

Order/Style No: — A8A6P Reporting Date: — 28/01/2024

Body Color: — Olive Testing Stage: — Sample

Print Type: — Rubber Print Sample Type: — Strike off

Print Color: — Applicant’s: — Mr. Alim

Fabric Type: — s/j Others: —

Report No: — VFN~SAM0500-0124A

TEST CONDUCTED

PRINT DURABILITY TEST—Appearance after washing/drying:

VFOI-004/AATCC 135 (Domestic washing)


(Machine wash at 40°C, Followed By Line Dry)
AATCC 1993 Standard Reference Detergent (WOB) 20g/wash, Using Miele, Wash inside out.

Observation After 01st Washing After 05th Washing After 10th Washing Requirement

Colour Change of Fabric 4-5 4-5 4-5

Colour Change of Print 4 3-4 3

Cracking No Cracking Observed No Cracking Observed No Cracking Observed


Class 4.0
Change of Surface Negligible Shade Change Observed Shade Change Observed

Appearance of Print Found Okay Found Not Okay Found Not Okay

Comments: After 01st, 05th, 10th time washes the overall print durability found as Not acceptable.

Final Result: Accepted Rejected √