JIS G3101-2004 Rolled steels for general structure

Tensile Test Chemical Compositions % Grade C SS330 0.050 max 0.050 max Mn P S Yield Point or Yield Strength N/mm2 Thickness (mm) t16 16t40 40t100 t100 205 min 245 min 285 min 0.30 max 1.60 max 0.040 max 0.040 max 400 min 195 min 235 min 275 min 390 min 175 min 215 min 255 min 165 min 205 min 245 min Tensile Strength N/mm2 Elongation Thickness (mm) 6t16 16t50 40t 6t16 16t50 40t 6t16 16t50 40t 6t16 16t40 Test Piece No.1A No.1A No.4 No.1A No.1A No.4 No.1A No.1A No.4 No.1A No.1A % (min) 21 26 28 17 21 23 15 19 21 13 17

330-430

SS400

400-510

SS490 SS540

490-610 540 min

Remark1.Alloy elements other than those shown in the above table may be added necessary. 2.For the elongation of No.4 test piece for steel plates over 90mm in thickness, it shall be subtracted 1% from the values of per each increase of 25mm or its fraction in thickness. However, the limit to be subtracted shall be 3%.