TEST REPORT no: RMNT19004197
Date: 01.11.2019

Sample received date: 28.10.2019 pm


Test start date: 29.10.2019 am

TEST REPORT

Applicant details:
Mantra SRL
Applicant:
str. Birsei nr.11 bis, Focsani, county Vrancea, Romania
Dan Isac
Contact person:
dan.isac@mantra.ro
Buyer’s name: LK Bennett
Description:
Your reference: JK+SK+ LOWRI
Order number: -
Specification: In accordance with LK Bennett Specification
Performance: Table 9.4 Woven Tailoring, Casual, Soft Dressing
End use: -
Season: -
One sample of green/multi woven fabric – Woven fabric for jacket and skirt - Art. 1691/A.027, col
Sample description:
002
Colour declared: col 002
Claimed to be: 62% cotton, 38% polyamide
Tests conducted: At applicant request

Provided care label:

Comments:

Prepared & checked by: Intertek ATI


For: LK BENNETT

Alina Calin Diana Balan


Coordinator Laboratory Manager

Intertek ATI is accredited in accordance with SR ISO/CEI 17025:2005, RENAR accreditation certificate: no. LI 904/ 2019. Opinion and interpretations
expressed herein are outside the scope of RENAR accreditation. Results and comments are valid only for the test samples that were submitted to the
textile laboratory Intertek ATI. They can not be extrapolated to the general proprieties of a batch.The copyright of that document is only authorized
under its integral form. Only the reports with national accreditation mark are inside the scope of Renar accreditation.
Nr. Reg.Com. J40/12/2005. Nr unic de Inreg:RO 17091186 Page 1 of 4
F-ITK-5.10-02
Intertek ATI Labtest
Calea Rahovei 266-268, Bucuresti
tel: 004021 404 81 48
romania.softlines@intertek.com
TEST REPORT no: RMNT19004197
Date: 01.11.2019

Test name Results Remarks


(^) Dimensional stability to dry cleaning P
Seam slippage F See results
Seam strength F See results
Tensile strength P
Tear strength NA See results
Abrasion Martindale P
Pilling resistance P
Fiber composition P
Flammability NA Weight exception
Color fastness to dry cleaning P
Color fastness to rubbing P
Color fastness to water F Nylon: 3/4
Colour fastness to perspiration P

P = Pass x = Did not perform


F = Fail NA = Not applicable
* = See remark NR = No specified requirement
SC = Still continues (^) = subcontracted test

Intertek ATI is accredited in accordance with SR ISO/CEI 17025:2005, RENAR accreditation certificate: no. LI 904/ 2019. Opinion and interpretations
expressed herein are outside the scope of RENAR accreditation. Results and comments are valid only for the test samples that were submitted to the
textile laboratory Intertek ATI. They can not be extrapolated to the general proprieties of a batch.The copyright of that document is only authorized
under its integral form. Only the reports with national accreditation mark are inside the scope of Renar accreditation.
Nr. Reg.Com. J40/12/2005. Nr unic de Inreg:RO 17091186 Page 2 of 4
F-ITK-5.10-02
Intertek ATI Labtest
Calea Rahovei 266-268, Bucuresti
tel: 004021 404 81 48
romania.softlines@intertek.com
TEST REPORT no: RMNT19004197
Date: 01.11.2019

Tests conducted (as requested of the applicant)

Test name Standards// Test method Results Requirements


+/-3%
Warp: -0.7%
SR EN ISO 3759:2011/ +/-5%
Dimensional stability Weft: -0.8%
(^)Commercial proces (Viscose/Knits)
to dry cleaning
Note: ( + ) means extension and ( - ) means shrinkage
(^) Dry cleaning process is subcontracted to a local commercial company.
SR EN ISO 13936-1: 2004
Conditioning atmosphere Standard seam
Jaw pressure: 100 N Warp seam: SO 6 mm@ 3.8 kg 8kg
Seam slippage
Test speed: 50 mm/min Weft seam: SO 6 mm@ 2.6 kg
No. of specimens tested: 8
Weight: 215 g/m2
SO=Seam Opening
SR EN ISO 13935-2: 2014
Conditioning atmosphere
Warp seam: 7.9 kg (TPO)
Jaw pressure: 100 N 12 kg
Seam strength Weft seam: 4.3 kg (TPO)
Test speed: 50 mm/min
No. of specimens tested: 8
Weight: 215 g/m2
Note: TPO =threads pull out
SR EN ISO 13934-2: 2014
Jaw pressure: 100 N
Warp: 26.0 kg
Tensile strength Test speed: 50 mm/min 15 kg
Weft: 32.8 kg
No. of specimens tested: 8
Weight: 215 g/m2
SR EN ISO 13937-1: 2001
Conditioning atmosphere Warp: incomplete tears
Tear strength 1000 g
Elmatear machine Weft: incomplete tears
Weight: 215 g/m2
SR EN ISO 12947-1,2, 4: 2006
Conditioning atmosphere
No broken threads @ 20000 revs. 15000 revs
Abrasion resistance Machine: Martindale
Color change 4/5 @ 5000 revs. 4 CC@ 5000 revs
Test pressure: 9 kPa
Test conducted until: 20000 revs.
SR EN ISO 12945-2: 2002
125 revs: 4
Conditioning atmosphere
500 revs: 3/4
Pilling Martindale After dry cleaning 3/4 @ 2000 revs
1000 revs: 3/4
M= 415 g
2000 revs: 3/4
Conducted to 2000 cycles
SR EN ISO 1833-1,4: 2011;
62.6% cotton 62% cotton
EU Regulation 1007: 2011
Fiber composition 37.4% polyamide 38% polyamide
Microscopic analysis and manual
separation Tolerance ±3%
As verified the sample is Exemption from
flammability testing in accordance with: 16 CFR Plain & raised
Flammability of
US CPSC 16 CFR §1610:2008 Part 1610.1 (d)(1): surface fabrics:
Clothing Textiles
Plain surface fabric with weight: 215 g/m2 // 6.34 Class 1
oz/yd2

Intertek ATI is accredited in accordance with SR ISO/CEI 17025:2005, RENAR accreditation certificate: no. LI 904/ 2019. Opinion and interpretations
expressed herein are outside the scope of RENAR accreditation. Results and comments are valid only for the test samples that were submitted to the
textile laboratory Intertek ATI. They can not be extrapolated to the general proprieties of a batch.The copyright of that document is only authorized
under its integral form. Only the reports with national accreditation mark are inside the scope of Renar accreditation.
Nr. Reg.Com. J40/12/2005. Nr unic de Inreg:RO 17091186 Page 3 of 4
F-ITK-5.10-02
Intertek ATI Labtest
Calea Rahovei 266-268, Bucuresti
tel: 004021 404 81 48
romania.softlines@intertek.com
TEST REPORT no: RMNT19004197
Date: 01.11.2019

Test name Standards// Test method Results Requirements


Colour change 4/5
Colour staining
Acetate 4/5
SR EN ISO 105 D01: 2013 Change: 4
Colour fastness to dry Cotton 4/5
Used solvent: Perchloroethylene Stain: 4
cleaning Nylon 4/5
Grey scale evaluation Cross Stain: 4/5
Polyester 4/5
Acrylic 4/5
Wool 4/5
Colour fastness to SR EN ISO 105 X12: 2016 Dry: 5 Dry: 4
rubbing Grey scale evaluation Wet: 4 Wet: 3/4
Colour change 4/5
Colour staining
Acetate 4/5
SR EN ISO 105 E01: 2013 Change: 4
Colour fastness to Cotton 4
4 hours @ 37± 2oC Stain: 4
water Nylon 3/4
Grey scale evaluation Cross stain: 4/5
Polyester 4
Acrylic 4/5
Wool 4/5
Colour change 4/5
SR EN ISO 105 E04: 2013 Colour staining
Alkaline
Acetate 4/5
Cotton 4
pH: 8.0 ±0.2
Nylon 4
Perspirometer: 4h @ (37±2)ºC;
Polyester 4/5
vertical position; 12.5 kPa
Grey scale evaluation Acrylic 4/5
Colour fastness to Change: 4
Wool 4/5
perspiration Stain: 4
Colour change 4/5
SR EN ISO 105 E04: 2013 Cross stain: 4/5
Colour staining
Acid
Acetate 4/5
Cotton 4
pH: 5.5±0.2
Nylon 4
Perspirometer: 4h @ (37±2)ºC;
Polyester 4/5
vertical position; 12.5 kPa
Grey scale evaluation Acrylic 4/5
Wool 4/5

KEYS
Explanation of Color Fastness Result
Grade 5: Negligible or no change or staining
Grade 4: Slightly changed or stained
Grade 3: Noticeably changed or stained
Grade 2: Considerably changed or stained
Grade 1: Much changed or heavily stained

END OF REPORT

This report is made solely on the basis of your instructions and /or information and materials supplied by you. It is not intended to be a
recommendation for any particular course of action. Intertek does not accept a duty of care or any other responsibility to any person other than the
Client in respect of this report and only accepts liability to the Client insofar as is expressly contained in the terms and conditions governing Intertek’s
provision of services to you. Intertek makes no warranties or representations either express or implied with respect to this report save as provided for
in those terms and conditions. We have aimed to conduct the Review on a diligent and careful basis and we do not accept any liability to you for any
loss arising out of or in connection with this report, in contact, tort, by statute or otherwise, except in the event of our gross negligence or willful
misconduct.

Intertek ATI is accredited in accordance with SR ISO/CEI 17025:2005, RENAR accreditation certificate: no. LI 904/ 2019. Opinion and interpretations
expressed herein are outside the scope of RENAR accreditation. Results and comments are valid only for the test samples that were submitted to the
textile laboratory Intertek ATI. They can not be extrapolated to the general proprieties of a batch.The copyright of that document is only authorized
under its integral form. Only the reports with national accreditation mark are inside the scope of Renar accreditation.
Nr. Reg.Com. J40/12/2005. Nr unic de Inreg:RO 17091186 Page 4 of 4
F-ITK-5.10-02

You might also like