You are on page 1of 1
fy a 18214 182M - 04 TABLE 1 Continued ‘ustenitzing/Souoning Cooling ‘Guerating Gaal Tempering Temperature, rede Heat Tet Type Temperature, nF °C)" Mea Below F (0) mF C0), Foo ‘elton Wat and quench 1900 [7040] aud 00 60) : aot Satuton eat and guenen 1800 [1040] qua 500 (260) 5 20d 4900 (040) que 500 (250) 5 088 18001040] ia 500 260) : S04 480 (040) qua 500 [260] 5 200H Seluton reat and quonen 1000 (1040) que 500 250) 5 Fat Selon reat and qvenen 1900 [1040] ua 500 260) : Eaton Salutonveat and quency 1800 (040) aud 500 (260) 5 310MoLN Seluton reat and quench 1000-2010 1050-1100) qu 500 250) 5 Fate Selon reat ana qvenen 1800 [1040] Fue 500 260) 5 Fate Seluton eat and quench 1800 [1040] aud 500 [260] 5 aire Seluton reat and quonen 10001040) que 500 (260) 5 F 3168 Selon reat and quenen 1900 [1040] us 500 (260) 5 ry Selutonveat and quencn 1800 [1040] aud 500 260) Fair felon rat and quonen 1000 (1040) que 500 260) 5 Fain, Selon reat and quench 1800 [1040] ud 500 (260) Fur Seluon eat and quencn 1800 (1040) qua 500 260) ar felon rat and quonen 2000 (1095) eu 500 260) Fe elon eat and quene 1900 [1040] ud 500 (260) Fae Seluton eat ana quancn 2000 (1095) qua 500 260) Fant 1900 (1040) que 500 (260) F 2H 2000 [1085] ud 500 260) Ewer 4800 (040) qua 500 260) FAM 1900 (1040) que 500 (260) Fi 1800 [1040] ud 500 (260) £20 4700-880 (0254010) tau 500 260) Fae 2100 (118) que 500 (260) Fas 1800 [1040] ud 500 (260) Fae 20102140 (100-1140) auld 500 260) Far 1800 1040) fue 500 (260) Fa 180 [1040] ud 500 260] Fa 2080 (112) qua 500 260) Fo 2080-2160 (120-1180) ld 500 (260) F58 2085 1140] ud 500 260) Fe 2025 1105) qua 500 260) Frc AustntyStairone Stole Feo elon eat and quench 1925 (7050) Tue 500 60) p Fst Selunon eat and quench 1870 [120] aud 500 [260] G Fae qua 500 280) 5 F53 selon reat and quened 1600 (1025) eu 500 (260) 5 Fo felon rat and quenen 18202060 (10504125) baud 500 [260] G Fos feluton rat and quench 20102085 [1100-140] aque 500 (250) 5 Fo Selon reat and quenes 1840 (1080) aud 17580) 5 Fe felon reat and quench 18752060 [1080-120] baud 500 (260) G Foo Salut rat and quenen 1870 (1020) qua 500 250) 5 For Selon eat and quenen 10202060 [1050-125] qu 500 (260) : Fou feluon rat and quench 19202400 1050-160] baud 500 (260) 2 ‘nimum unless temperate range listed. * Not appeal © Grade F 52 shall be soktion este at 1625 to 1875°F [9 to 1025°] 30 iin. of hkness and water quenched 7. Chemical Composition 7.1 A chemical heat analysis in accordance with Specifica- tion A961 shall be made and conform to the chemical ‘composition prescribed in Table 2. 7.2 Grades to which lead, selenium, or other elements are added for the purpose of rendering the material free-machining shall not be used. 7.3 Starting material produced to a specification that spe- cifically requires the addition of any element beyond those listed in Table 2 for the applicable grade of material is not permitted "74 Stainless steel grades covered in this specification shall not contain an unspecified clement, other than nitrogen, for the ordered grade to the extent that the steel conforms to the requirements of another grade for which that clement is @ specified element having a required minimum content. For this requirement, a grade is defined as an alloy deseribed individu- ally and identified by its own UNS designation in Table 2 of Chemical Requirements with being covered by this specifica- tion. 175 Product Analysis—The purchaser may make a product analysis on products supplied to this specification in accor- dance with Specification A 961

You might also like