You are on page 1of 7

Aldoksan Alloys Casting Alloy Properties

Alloy Designation C61400 Cu Al Fe Mn


Chemical Composition CW303G rem. 6.0-8.0% 1.5-3.5% 1.0%
Typical Mechanical Properties Tensile Strength Yield Strength Elongation %
metric Mpa 540-570 220-270 34-40
imperial Ksi 78-83 32-38 34-40
Typical Physical Properties Density Specific Heat Electrical Conductivity Thermal Conductivity
metric 7.89 gm/cm3 377.1 J/kg-K 0.082 MegaSiemens/cm 67.5 W/m-K
imperial 0.285 lb/in3 0.09 BTU/lb 14 %IACS 39.0 BTU/h-ft-°F

Alloy Designation C63000 Cu Al Ni Fe Mn Zn


Chemical Composition AMS4640 rem. 9.0-11.0 4.0-5.5 2.0-4.0 1.5 max 0.3 max
Typical Mechanical Properties Tensile Strength Yield Strength Elongation % Hardness Brinell
metric MPa 600-770 300-400 12-20 180-240
imperial Ksi 87.0-111.7 43.5-58.0 12-20 180-240
Typical Physical Properties Density Specific Heat Electrical Conductivity Thermal Conductivity
metric 7580 kg/m³ 376.7 J/kg-K 0.041 Mega Siemens/cm 39.1 W/m-K
imperial 0.274 lb/in³ 0.090 Btu/lb 7% IACS 22.6 BTU/h-ft-°F

Alloy Designation C63020 Cu Al Ni Fe Mn Zn


Chemical Composition AMS4590 rem. 10.0-11.0 4.2-6.0 4.0-5.5 1.5 0.3
Typical Mechanical Properties Tensile Strength Yield Strength Elongation % Hardness Brinell
metric Mpa 800 570 4 215
imperial Ksi 135 100 4 215
Typical Physical Properties Density Specific Heat Electrical Conductivity Thermal Conductivity
metric 7.6 gm/cm3 450 J/kg-K 54 W/m-K
imperial 0.269 lb/in³ 0.11 Btu/lb 6 %IACS 0.11 BTU/h-ft-°F

Alloy Designation C63200 Cu Al Ni Fe Mn


Chemical Composition rem. 8.7-9.5 4.0-4.8 3.5-4.3 1.2-2.0
Typical Mechanical Properties Tensile Strength Mpa Yield Strength Mpa Elongation % Hardness Brinell
metric MPa 621-738 345-386 15-23 190-230
imperial Ksi 90-107 50-56 15-23 190-230
Typical Physical Properties Density Specific Heat Electrical Conductivity Thermal Conductivity
metric 7640 kg/m³ @ 20ºC 439 J/kg-K 0.041 Mega Siemens/cm 34.6 W/m-K
imperial 0.276 lb/in³ 0.105 Btu/lb 7 % IACS 20 BTU/h-ft-°F
Aldoksan Alloys Casting Alloy Properties

Alloy Designation C70600 Cu Al Ni Fe Mn Zn


Chemical Composition CUNI10 rem. 9.0-11.0 1.0-1.8 1 1
Typical Mechanical Properties Tensile Strength Yield Strength Elongation % Hardness Brinell
metric Mpa 370 164 45 85
imperial Ksi 80-60 16-57 45 85
Typical Physical Properties Density Specific Heat Electrical Conductivity Thermal Conductivity
metric 8.94 gm/cm3 377.1 J/kg-K 0.053 MegaSiemens/cm 45.0 W/m-K
imperial 0.323 lb/in3 0.09 Btu/lb 9 %IACS 26.0 BTU/h-ft-°F

Alloy Designation C71500 Cu Al Ni Fe Mn Zn


Chemical Composition CUNI30 rem. 29.0-33.0 0.4-1.0 1 1
Typical Mechanical Properties Tensile Strength Yield Strength Elongation % Izod (Joules)
metric Mpa 310-360 110-140 30-40 54-100
imperial Ksi 54-75 20-70 30-40 54-100
Typical Physical Properties Density Specific Heat Electrical Conductivity Thermal Conductivity
metric 8.94 gm/cm3 377.1 J/kg-K 0.027 MegaSiemens/cm 29.4 W/m-K
imperial 0.323 lb/in3 0.09 Btu/lb 4 %IACS 17.0 BTU/h-ft-°F

Alloy Designation C86300 Cu Al Ni Fe Mn Zn


Chemical Composition AMS4855 60.0-66.0% 5.0-7.5% 1.0% 2.0-4.0% 2.5-5.0% 22.0-28.0%
Typical Mechanical Properties Tensile Strength Yield Strength Elongation % Hardness Brinell
metric Mpa 850 480 14 250
imperial Ksi 120 69 14 250
Typical Physical Properties Density Specific Heat Electrical Conductivity Thermal Conductivity
metric 7.83 gm/cm3 377.1 J/kg-K 0.0746 MegaSiemens/cm 35.5 W/m-K
imperial 0.283 lb/in3 0.09 BTU/lb 8.0 %IACS 20.5 BTU/h-ft-°F

Alloy Designation C95400 Cu Al Ni Fe Mn


Chemical Composition rem. 10.0-11.5 3.0-5.0 0.5
Typical Mechanical Properties Tensile Strength Yield Strength Elongation % Hardness Brinell
metric Mpa 590 230 12 150
imperial Ksi 75-85 30-32 12 150
Typical Physical Properties Density Specific Heat Electrical Conductivity Thermal Conductivity
metric 7.45 gm/cm3 420 J/kg-K 0.75 MegaSiemens/cm 58.7 W/m-K
imperial 0.269 lb/in3 0.1 Btu/lb 13 % IACS 33.9 BTU/h-ft-°F
Aldoksan Alloys Casting Alloy Properties

Alloy Designation C95500 Cu Al Ni Fe Mn


Chemical Composition 78.0 min% 10.0-11.5% 3.0-5.5% 3.0-5.0% 3.5%
Typical Mechanical Properties Tensile Strength Yield Strength Elongation % Hardness Brinell
metric Mpa 700-850 320-470 8.4-10.0 200-210
imperial Ksi 100-120 46-69 8.4-10.0 200-210
Typical Physical Properties Density Specific Heat Electrical Conductivity Thermal Conductivity
metric 7.53 gm/cm3 419.0 J/kg-K 0.049 MegaSiemens/cm 41.9 W/m-K
imperial 0.272 lb/in3 0.1 BTU/lb 8 %IACS 24.2 BTU/h-ft-°F

Alloy Designation C95510 Cu Al Ni Fe


Chemical Composition AMS4880 rem. 10.3 5 2.7
Typical Mechanical Properties Tensile Strength Yield Strength Elongation % Hardness Brinell
metric Mpa 655-780 386-460 9-12 175-240
imperial Ksi 95-113 56-67 9-12 175-240
Typical Physical Properties Density Specific Heat Electrical Conductivity Thermal Conductivity
metric 7.53 gm/cm3 376.7 J/kg-K 0.049 MegaSiemens/cm 41.9 W/m-K
imperial 0.272 lb/in3 0.090 Btu/lb 8.5 %IACS 24.2 BTU/h-ft-°F

Alloy Designation C95520 Cu Al Ni Fe Mn Zn


Chemical Composition AMS4881 rem 10.5-11.5 4.2-6.0 4.0-5.5 1.5 0.3
Typical Mechanical Properties Tensile Strength Yield Strength Elongation % Hardness Brinell
metric Mpa 890-930 630-725 2 262
imperial Ksi 135 100 2 262
Typical Physical Properties Density Specific Heat Electrical Conductivity Thermal Conductivity
metric 8.2 gm/cm3 450 J/kg-K 40 W/m-K
imperial 0.510 lb/in3 0.11 BTU/lb 8.5 %IACS 24.2 BTU/h-ft-°F

Alloy Designation C95800 Cu Al Ni Fe Mn


Chemical Composition rem. 8.5-9.5 4.0-5.0 3.5-4.5 0.8-1.5
Typical Mechanical Properties Tensile Strength Yield Strength Elongation % Hardness Brinell
metric Mpa 590 250 18 159
imperial Ksi 85 35 18 159
Typical Physical Properties Density Specific Heat Electrical Conductivity Thermal Conductivity
metric 7.64 gm/cm3 440.0 J/kg-K 0.041 MegaSiemens/cm 36 W/m-K
imperial 0.276 lb/in3 0.105 Btu/lb % 7 IACS 250 BTU in/hr.ft².°F
Aldoksan Alloys Casting Alloy Properties

Alloy Designation UN14A2 Cu Al Ni Fe


Chemical Composition CuNi14Al2 rem. 3 14
Typical Mechanical Properties Tensile Strength Yield Strength Elongation % Hardness Brinell
metric Mpa 1000 750 12 250
imperial Ksi 145 109 12 250
Typical Physical Properties Density Specific Heat Electrical Conductivity Thermal Conductivity
metric 8.7 gm/cm3 0.416 J/(g.°K) 11 71 W/m-K
imperial 0.307 lb/in3 0.0993 Btu/lb 11 41.1 BTU/h-ft-°F

Alloy Designation UZ19A6 Cu Al Ni Fe Mn Zn


Chemical Composition NFL14707 rem. 6.5 3 5.5 18.5
Typical Mechanical Properties Tensile Strength Yield Strength Elongation % Hardness Brinell
metric Mpa 780-830 540-590 7-10 225
Typical Physical Properties Density Specific Heat Electrical Conductivity Thermal Conductivity
7.6 gm/cm3 6 %IACS 35 W/m-K

Alloy Designation UA11N Cu Al Ni Fe Mn


Chemical Composition NFL14706 77.8% 10.7% 5.3% 5.3% 0.9%
Typical Mechanical Properties Tensile Strength Yield Strength Elongation % Hardness Brinell
metric Mpa 690-760 320-400 10 179-255
Typical Physical Properties Density Specific Heat Electrical Resistivity Thermal Conductivity
metric 7.6 gm/cm3 22 μΩ.m15°C 54 W/m-K
Aldoksan Alloys Casting Hard Bronze Alloy Properties

Alloy Designation ALBA280 Cu Al Fe Others


Chemical Composition rem. 12.8-13.4% 4.2-4.6% 2.5 max%
Typical Mechanical Properties Tensile Strength Yield Strength Elongation % Hardness Brinell
metric Mpa 517 379 1.5 260-286
Typical Physical Properties Density Specific Heat Electrical Conductivity Thermal Conductivity
7.2 gm/cm3 0.42 J/kg-K 10 %IACS 42 W/m-K

Alloy Designation ALBA310 Cu Al Fe Mn Others


Chemical Composition rem. 14.5% 4.5% 2.0% 0.2%
Typical Mechanical Properties Tensile Strength Yield Strength Elongation % Hardness Brinell
metric Mpa 586 489 0.5 310-332
Typical Physical Properties Density Specific Heat Electrical Conductivity Thermal Conductivity
7.06 gm/cm3 0.42 J/kg-K 10 %IACS 42 W/m-K

Alloy Designation ALBA360 Cu Al Fe Mn Others


Chemical Composition - - - - -
Typical Mechanical Properties Tensile Strength Yield Strength Elongation % Hardness Brinell
metric Mpa 1500 689 0 340-375
Typical Physical Properties Density Specific Heat Electrical Conductivity Thermal Conductivity
6.93 gm/cm3 0.42 J/kg-K 8 %IACS 33 W/m-K

Alloy Designation ALBA390 Cu Al Fe Mn Others


Chemical Composition - - - - -
Typical Mechanical Properties Tensile Strength Yield Strength Elongation % Hardness Brinell
metric Mpa 1515 689 0 400-420
Typical Physical Properties Density Specific Heat Electrical Conductivity Thermal Conductivity
6.84 gm/cm3 0.42 J/kg-K 8 %IACS 33 W/m-K
Aldoksan Alloys Casting Resistance Welding Alloy Properties

Alloy Designation C17200 CuBe2 Cu Be Co Al


Chemical Composition AMS4533 AB44 rem. 1.8-2.0% 0.2 min% 0.2%
Typical Mechanical Properties Tensile Strength Yield Strength Elongation % Hardness Brinell
metric Mpa 480-1380 160-1250 1.1-37 340
imperial Ksi 70-200 23-180 1.1-37 340
Typical Physical Properties Density Specific Heat Electrical Conductivity Thermal Conductivity
metric 8.25 gm/cm3 419.0 J/kg-K 0.129 MegaSiemens/cm 107.3 W/m-K
imperial 0.298 lb/in3 0.1 BTU/lb 22 %IACS 62.0 BTU/h-ft-°F

Alloy Designation CW103C CuCoNiBe Cu Be Co Ni Others


Chemical Composition AB4 rem. 0.5% 1.1% 1.1% 0.2%
Typical Mechanical Properties Tensile Strength Yield Strength Elongation % Hardness Brinell
metric Mpa 700-800 500-600 8 220-260
Typical Physical Properties Density Specific Heat Electrical Conductivity Thermal Conductivity
metric 8.8 gm/cm3 0.42 J/kg-K 24-30 MegaSiemens/cm 230 W/m-K

Alloy Designation C17500 CuCo2Be Cu Be Co Si - Al


Chemical Composition CW104C AC4 rem. 0.4-0.7% 2.4-2.7% 0.2% - 0.2%
Typical Mechanical Properties Tensile Strength Yield Strength Elongation % Hardness Brinell
metric Mpa 700-800 500-600 8 220
Typical Physical Properties Density Specific Heat Electrical Conductivity Thermal Conductivity
metric 8.8 gm/cm3 0.40 J/kg-K 26-30MegaSiemens/cm 230 W/m-K

Alloy Designation C17510 CuNi2Be Cu Be Co Ni Si - Al


Chemical Composition CW110C AN4 rem. 0.2-0.6% 0.3% 1.4-2.2% 0.2% - 0.2%
Typical Mechanical Properties Tensile Strength Yield Strength Elongation % Hardness Brinell
metric Mpa 640-760 500-650 8 250-280
Typical Physical Properties Density Specific Heat Electrical Conductivity Thermal Conductivity
metric 8.86 gm/cm3 0.40 J/kg-K 30 MegaSiemens/cm 210-310 W/m-K

Alloy Designation C18000 CuNi3SiCr Cu Ni Si Cr Others


Chemical Composition AN3S rem. 2.4% 0.7% 0.4% 0.2%
Typical Mechanical Properties Tensile Strength Yield Strength Elongation % Hardness Brinell
metric Mpa 600-700 450-500 5 180-220
Typical Physical Properties Density Specific Heat Electrical Conductivity Thermal Conductivity
metric 8.7 gm/cm3 0.38 J/kg-K 26-28 MegaSiemens/cm 208 W/m-K
Aldoksan Alloys Casting Resistance Welding Alloy Properties

Alloy Designation C18150 CuCrZr Cu Cr Zr Fe - Si - Pb Others


Chemical Composition AC1Z rem. 0.3-1.2% 0.03-0.3% 0.05% - 0.05% - 0.05% 0.1 max%
Typical Mechanical Properties Tensile Strength Yield Strength Elongation % Hardness Brinell
metric Mpa 370-450 270-350 10-22 135
Typical Physical Properties Density Specific Heat Electrical Conductivity Thermal Conductivity
metric 8.9 gm/cm3 0.38 J/kg-K 44-49 MegaSiemens/cm 320 W/m-K

Alloy Designation C18200 CuCr1 Cu Cr Others


Chemical Composition AC1 rem. 1.0% 0.2%
Typical Mechanical Properties Tensile Strength Yield Strength Elongation % Hardness Brinell
metric Mpa 485 450 18 135
Typical Physical Properties Density Specific Heat Electrical Conductivity Thermal Conductivity
metric 8.9 gm/cm3 0.38 J/kg-K 49-51 MegaSiemens/cm 320 W/m-K