lead Oe
PT. PAMOLITE ADHESIVE INDUSTRY
Prone: (0935) 421884 = Hasing
ex (0535/4220,
‘Attn : Bpk. Sandy
Date of Received
Date of Test
Date of Product
Product & Type
Quantity / Size / Thickness
REPORT OF TESTING
No ; 1367/PAVPROB/XI/20
December 4, 2020
December 7-8, 2020
December 2,2020
Plywood All Sengon Type 2 EO
9 Pes /40 em x $0 em /17,5 mm
Tested for Delamination, Bonding strength, Emission & Moisture Content
‘Standard Test Method JAS- 2014
Company ‘
Address Malang,
Result Classification.
Delamination ation Delamination
SempleCode [1 [2 | 3 | 4 [Rewt More Than 90%
17S mm/Kanan_|o [0 | 0 | 0 | 100%] Passed
1Smm/Kid [0 [0 | 0 | 0 | 100%] Passed
TSem Tengah [0 [0 | 0 | 0 | 100%] Passed
Bonding Strengtit
‘Chasiieation Bonding Strength
Sample Code [Max (Wmm{ Min (Nimmi] Avg (Vina) Species Of Vencer | Bonding Strength | Avg Wood Failure
V7 mm Kanan [0,74 (10) | 0,71 (10) | 0.72 (10) | Passed] | Hard wood | Min. 0.70 Nim?
17S mm/Ki | 1,02_(20)| 0.71 (40) | 0.83 G0) | Passed Min, 0.60 Ninn 50%
T7Sam/ Teagan [0,75 (10) | 0.71 0) | 0.73 (10) | Passed} | Soft Wood [ Min. 0.50 Nimm™ om
Min. 040 Ninn 30%
Enisson ‘Classification Emission
‘Sample Code mg (oem) Category ‘Avg ( mg/L) Max (mg)
17S mm Kanan 030, Benes 030 0.40
17S wm Kie 029 Pre 0,70
17 mm / Tenge 031 Fe 210
‘Average 030 re 7,00
Max 031
Category Pee
Moisture Content ‘Chassification Moisture Content of Piywood
‘Sample Code Result (6) Less Than 14%:
TS mm / Kanan 0.00
17S mm Kirk 10,00
1.8 mm Tengah 10.00
Probolinggo, December 15, 2020
Manager