RETUBING 170-WHB-2

PT.PERTAMINA (PERSERO) RU-II DUMAI


Rejection Welder AS per 15/01/2018

Radiography Film Of Radiography Rejection KIND OF DEFECT RADIOGRAPHY ( Film )


Welder No Rate
Total Repair Total Acc Defect
Cr LOF IP P TI UC SL RC IF SI Si Cp Orther Total
Joint Joint Film Film Film %
W-01 0 0 0 0 0 #DIV/0! 0 0 0 0 0 0 0 0 0 0 0 0 0 0
W-02 142 0 291 284 7 2% 0 0 0 2 0 0 0 0 5 0 0 0 0 7
W-03 166 0 346 332 14 4% 0 0 0 7 0 0 0 0 5 0 0 0 0 12
W-04 88 1 161 150 11 7% 0 0 0 8 0 0 0 0 0 0 0 0 0 8
W-05 0 0 0 0 0 #DIV/0! 0 0 0 0 0 0 0 0 0 0 0 0 0 0
W-06 0 0 0 0 0 #DIV/0! 0 0 0 0 0 0 0 0 0 0 0 0 0 0

Total 396 1 798 766 32 4% 0 0 0 17 0 0 0 0 10 0 0 0 0 27

Ket : List Welder :


Cr : Crack Si : Slag Inclution W-01 : Mohammad Darsam
Lof : Lack Of Fusion CP : Cluster Porosity W-02 : Solikin
IP : Incomplete Penetration W-03 : Yeyen Sugianto
P : Porosity W-04 : Abdul Rahman
TI : Tungsten Inclution W-05 : Mustain
Uc : Under Cut W-06 : M. Hakim
Sl : Slag Line
Rc : Root Concavity
IF : Incomplete Fusion
Sl : Surface Indication