PK335

DIN Material No. Code Comparable standards Chemical composition ( Tipical analysis % ) Steel properties 1.2316 X36CrMo17 EU: X38CrMo 16 1 C 0.38 Cr 16.0 Mo 1.15

Stainless cold work tool steel. Good polishability.

Physical properties

Thermal conductivity W/(mK) Density g/cm3 Coefficient of linear thermal expansion 10-6 C-1
20-100 10.7 20-200 11.7 20-300 11.7 20-400 11.7

20 C 15 20 C 7.71
20-500 11.8 20-600 11.9 20-700 12.4 20-800 C 12.9

Applications Heat treatment

Dies for pressing chemically agressive compounds. Soft annealing C 790 - 840 Hardening from C 1000 - 1040 Tempering C HRC Cooling furnace in oil, thermal bath 500 550 C
49 47 46

Hardness HB max. 250 Hardness after quenching HRC 49 500 600


47 32

100 200 300 400


46

Time Temperature Transformation - Diagram

Tempering Diagram

70 65 60 Hardness in HRC 55 50 45 40 35 30 0 100 200 300 400 500 600 o Tempering Temperature in C, Time 1.5 h 700