S355 European Standard Steel


S355 EN 10025 : 2004 Standard Structural Steel Plate
S355 structural steel plate is a high-strength low-alloy European standard structural steel covering four of the six
"Parts" within the EN 10025 – 2004 standard. With minimum yield of 50,000 KSI, it meets requirements in chemistry
and physical properties similar to ASTM A572 / 709. Careful attention should always be placed on the specific
variation of S355 required if considering substitute material.

S355 is used in almost every facet of structural fabrication. Typical applications include:

 Structural steelworks: bridge components, components for offshore structures


 Power plants
 Mining and earth-moving equipment
 Load-handling equipment
 Wind tower components

Part 2 - Non-Alloy Structural Steels

S… Structural Steel

E... Engineering Steel

355 Minimum yield strength (Reh) in Mpa up to 16mm

…JR.. Charpy V-notch (Longitudinal) 27 J @ +20 Celsius

…JO.. Charpy V-notch (Longitudinal) 27 J @ 0 Celsius

…J2.. Charpy V-notch (Longitudinal) 27 J @ -20 Celsius

…K2.. Charpy V-notch (Longitudinal) 40 J @ +20 Celsius

…+AR Supply condition "As Rolled"

...+N Supply condition "Normalized or Normalized Rolled"

Additional Options

Grade with improved properties perpendicular to the surface


…Z..

   
2(7) 
 
Part 3 - Normalised / Normalised Rolled Weldable Fine Grain Structural Steel

S… Structural Steel

355 Minimum yield strength (Reh) in Mpa up to 16mm

...N.. Longitudinal Charpy V-notch impacts at a temperature not lower than minus 20 Celsius

...NL.. Longitudinal Charpy V-notch impacts at a temperature not lower than minus 50 Celsius

Additional Options

…Z.. Grade with improved properties perpendicular to the surface

Part 4 - Thermomechanically Rolled Weldable Fine Grain Structural Steels

S… Structural Steel

355 Minimum yield strength (Reh) in Mpa up to 16mm

...M.. Longitudinal Charpy V-notch impacts at a temperature not lower than minus 20 Celsius

...ML.. Longitudinal Charpy V-notch impacts at a temperature not lower than minus 50 Celsius

Additional Options

…Z.. Grade with improved properties perpendicular to the surface

   
3(7) 
 
Part 4 - Thermomechanically Rolled Weldable Fine Grain Structural Steels

S… Structural Steel

355 Minimum yield strength (Reh) in Mpa up to 16mm

…JO.. Charpy V-notch (Longitudinal) 27 J @ 0 Celsius

…J2.. Charpy V-notch (Longitudinal) 27 J @ -20 Celsius

…K2.. Charpy V-notch (Longitudinal) 40 J @ +20 Celsius

...W.. Improved Atmospheric Corrosion Resistance

...P.. Greater phosphorus content (grade S355 only)

...+AR Supply condition "As Rolled"

...+N Supply condition "Normalized or Normalized Rolled"

Additional Options

…Z.. Grade with improved properties perpendicular to the surface

(1MPa =
Mechanical Properties
145.03 PSI)

Grade Yield Strength (Mpa) in Nom. Thicknesses (mm)

>3 - >16 - >40 - >63- >80 - >100 - >150 - >200 - >250 -


<16 <40 <63 <80 <100 <150 <200 <250 <400

355 345 335 325 295 285 275


S355JR 315 min. -
min. min. min. min. min. min. min.

355 345 335 325 295 285 275


S355JO 315 min. -
min. min. min. min. min. min. min.

355 345 335 325 295 285 275 265


S355J2 315 min.
min. min. min. min. min. min. min. min.

355 345 335 325 295 285 275 265


S355K2 315 min.
min. min. min. min. min. min. min. min.

355 345 335 325 295 285 275


S355N 315 min.
min. min. min. min. min. min. min.

355 345 335 325 295 285 275


S355NL 315 min.
min. min. min. min. min. min. min.
4(7) 
 
(1MPa =
Mechanical Properties
145.03 PSI)

355 345 335 325 295


S355M 325 min.
min. min. min. min. min.

355 345 335 325 295


S355ML 325 min.
min. min. min. min. min.

355 345
S355J0WP - - - -
min. min.

355 345
S355J2WP - - - -
min. min.

355 345 335 325 295


S355J0W 315 min.
min. min. min. min. min.

Grade Tensile Strength (Mpa) in Nom. Thicknesses (mm)

>3 - >16 - >40 - >63- >80 - >100 - >150 - >200 - >250 -


<16 <40 <63 <80 <100 <150 <200 <250 <400

470 - 470 - 470 - 470 - 450 - 450 - 450 -


S355JR 470 - 630 -
630 630 630 630 600 600 600

470 - 470 - 470 - 470 - 450 - 450 - 450 -


S355JO 470 - 630 -
630 630 630 630 600 600 600

470 - 470 - 470 - 470 - 450 - 450 - 450 - 450 -


S355J2 470 - 630
630 630 630 630 600 600 600 600

470 - 470 - 470 - 470 - 450 - 450 - 450 - 450 -


S355K2 470 - 630
630 630 630 630 600 600 600 600

470 - 470 - 470 - 470 - 450 - 450 - 450 -


S355N 470 - 630 -
630 630 630 630 600 600 600

470 - 470 - 470 - 470 - 450 - 450 - 450 -


S355NL 470 - 630 -
630 630 630 630 600 600 600

470 - 470 - 450 - 440 - 430 -


S355M 440 - 600 - - -
630 630 610 600 590

470 - 470 - 450 - 440 - 325 440 - 430 -


S355ML - - -
630 630 610 600 600. 590

470 - 470 -
S355J0WP - - - - - - -
630 630

470 - 470 -
S355J2WP - - - - - - -
630 630
5(7) 
 
(1MPa =
Mechanical Properties
145.03 PSI)

470 - 470 - 470 - 470 - 450 -


S355J0W 470 - 630 - - -
630 630 630 630 600

Chemical Composition

Thickness
Grade C Mn P S Si Cr Ni Mo V Al Cu Ti Nb N
(mm)

.24 1.60 .035 .035 .55 .55 .012


S355JR <40 - - - - - - -
max max max max max max max

.24 1.60 .035 .035 .55 .55 .012


S355JR 41 - <150 - - - - - - -
max max max max max max max

151 - .24 1.60 .035 .035 .55 .55 .012


S355JR - - - - - - -
<250 max max max max max max max

.20 1.60 .030 .030 .55 .55 .012


S355JO <40 - - - - - - -
max max max max max max max

.22 1.60 .030 .030 .55 .55 .012


S355JO 41 - <150 - - - - - - -
max max max max max max max

151 - .22 1.60 .030 .030 .55 .55 .012


S355JO - - - - - - -
<250 max max max max max max max

.20 1.60 .025 .025 .55 .55


S355J2 <40 - - - - - - - -
max max max max max max

.22 1.60 .025 .025 .55 .55


S355J2 41 - <150 - - - - - - - -
max max max max max max

151 - .22 1.60 .025 .025 .55 .55


S355J2 - - - - - - - -
<250 max max max max max max

>250 - .22 1.60 .025 .025 .55 .55


S355J2 - - - - - - - -
<400 max max max max max max

.20 1.60 .025 .025 .55 .55


S355K2 <40 - - - - - - - -
max max max max max max

.22 1.60 .025 .025 .55 .55


S355K2 41 - <150 - - - - - - - -
max max max max max max

151 - .22 1.60 .025 .025 .55 .55


S355K2 - - - - - - - -
<250 max max max max max max
6(7) 
 
Chemical Composition

>250 - .22 1.60 .025 .025 .55 .55


S355K2 - - - - - - - -
<400 max max max max max max

.90
.20 .030 .025 .50 .030 .50 .10 .12 .02 .55 .05 .05 .015
S355N <250 -
max max max max max max max max min max max max max
1.65

.90
.18 .025 .020 .50 .030 .50 .10 .12 .02 .55 .05 .05 .015
S355NL <250 -
max max max max max max max max min max max max max
1.65

.14 1.60 .030 .025 .50 .030 .50 .10 .10 .02 .55 .05 .05 .015
S355M <150
max max max max max max max max max min max max max max

.14 1.60 .025 .020 .50 .030 .50 .10 .10 .02 .55 .05 .05 .015
S355ML <150
max max max max max max max max max min max max max max

.06 .25
.12 1.0 .035 .75 .009
S355J0WP <40 - - - - - - - -
max max max max max
.15 .55

.06 .25
.12 1.0 .030 .75
S355J2WP <40 - - - - - - - - -
max max max max
.15 .55

.50 .25
.16 .035 .035 .50 .009
S355J0W <150 - - - - - - - -
max max max max max
1.50 .55

Charpy V-Notch Testing

Elongation in Nom. Thicknesses (mm)

>3 >16 >40 >63 >80 >100 >150 >200 >250 Min.
@
Grade - - - - - - - - - Grain Absorbed
Degrees
<16 <40 <63 <80 <100 <150 <200 <250 <400 Energy

21 18
22 min +20
S355JR min 20 min (L) min 17 min (L) - - >27 J
(L) Celsius
(L) (L)

21 18
22 min 0
S355JO min 20 min (L) min 17 min (L) - - 27 J
(L) Celsius
(L) (L)

22 min -20
S355J2 21 20 min (L) 18 17 min (L) - 27 J
(L) Celsius
min min
7(7) 
 
Charpy V-Notch Testing

(L) (L)

21 18
22 min -20
S355K2 min 20 min (L) min 17 min (L) - 40 J
(L) Celsius
(L) (L)

22 min -20
S355N 21 min (Longitudinal) - 6 min 40 J
(Longitudinal) Celsius

22 min -50
S355NL 21 min (Longitudinal) - 6 min 27 J
(Longitudinal) Celsius

-20
S355M 22 min (Longitudinal) - - - 6 min 40 J
Celsius

-50
S355ML 22 min (Longitudinal) - - - 6 min 27 J
Celsius

22 min 0
S355J0WP - - - - - - - - 27 J
(L) Celsius

22 min -20
S355J2WP - - - - - - - - 27 J
(L) Celsius

18
0
S355J0W 20 min (Longitudinal) min - - - - 27 J
Celsius
(L)