Professional Documents
Culture Documents
To
Area 159.580 mm
Width 20.2 mm
Thickness = 7.9 mm
Gauge Length: 71 mm Final Gauge Length: 93.6 mm
Results of Tension Test
Maximum Force (Fm) 64,320.000 N
Yield Stress 241.008 N/mm
Disp. at Fm 51.300 mm
UTSYS Ratio 1.672
Max Disp. :63.800 mm
Tensile Strength (Rm): 403.058 N/mm
'Elongation :31.831 %
Yield Load
38,460.000N
Note: Yield Calculated By Offset method as per ASTM E8 at 5% Strain offset
Graph Stress Vs Strain
500.000
450.000
400.000
350.000
300.000
N
250.000
Stress 200.0
N/mm O
150.000
100.000
50.000
YO-0.000 9.000 18.000 7.000 36.000 45.000 54.000 63.000 72.000 81.000 90.000
0-0.000 -Strain %
colulilona
R.CD1
(SPIAL) OLKATA
Test Certificate
Name of Company Inspection Survey and Surveillance (lndia) Pt. Ltd.
Address Dum Dum. Kolkata
To
Sample ldentification 8 MM
THICK PLATE
Machine :FIE Make Universal
Testing Machine, UTE-60
Input Data :File Name: A-93495-09-05-B-1. Record No. 2, Date:
17-05-2022
Sample Type-- Rectangular Bar Area: 159.580 mm
Width 20.2 mm
Thickness =7.9 mm
:Gauge Length: 71 mm Final Gauge Length: 92.4 mm
500.000
450.000
400.000
350.000
300.000
250.000
Stress 200.000
N/mm
150.000
100.0
50.000
YO=0.000 8.000 16.000 24.000 32.000 40000 48.000 56.000 64.000 72.000 80.000
X0=0.000 -Strain%
7/0s/22
Nution ,
.c.D 1 9 . 01
, 01