Professional Documents
Culture Documents
A DESIGN CHARACTERISTIC
1-1 Designed compressive strength : C32Mpa (28days)
1-2 Sample size : Cylender sample 150 x 300
1
1-3 Ratio W/C : 0.45
1-4 S/A : 0.55
2-1 Cement ASTM type 1 : ASTM type I , K-Cement
2
2-2 Cement mass density : 3.14 g/cm3
3-1 Fine aggreegrate (Sand) : Sand (Model: 2.2)
3 3-2 Sand mass density Fine-Sand : 2.61 g/cm3
3-3 Sand mass density Coars-Sand : - g/cm3
4-1 Coars Aggregate (Crushed stone) : Crushed stone 10 x 20mm
4 4-2 Stone mass density : 2.71 g/cm3
4-3 Dmax : 25 mm
5-1 Chemical admixture : Sika Waterproof
5-2 Admixture dosage : Sika Plastocrete N 0.45 Kg/100kg of cement
5-3 Admixture dosage : Sika 771 1 Kg/100kg of cement
5
5-4 Admixture water-reducing 15% :
6-1 Admixture density : Sika Plastocrete N 1.170 g/cm3
6-2 Admixture density : Sika 771 1.136 g/cm3
6 6-3 Slump : 16 ± 2 Cm
3
B MIX-PROPORTION PER 1M
Note: Water
Mixing Reducing
by dry weight
15%
PREPARED BY WINESSED BY SIKA COMPANY APPROVED BY