You are on page 1of 2

Novodur® P2HGV

ABS-GF16 Styrolution

GF reinforced (16 %)
Rheological properties Value Unit Test Standard
ISO Data
Melt volume-flow rate, MVR 3 cm³/10min ISO 1133
Temperature 220 °C ISO 1133
Load 10 kg ISO 1133

Mechanical Properties Value Unit Test Standard


ISO Data
Tensile Modulus 5500 MPa ISO 527-1/-2
Yield stress 74 MPa ISO 527-1/-2
Yield strain 2 % ISO 527-1/-2
Charpy impact strength (+23°C) 18 kJ/m² ISO 179/1eU
Charpy impact strength, -30°C 20 kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) 6 kJ/m² ISO 179/1eA
Charpy notched impact strength, -30°C 5 kJ/m² ISO 179/1eA

Thermal Properties Value Unit Test Standard


ISO Data
Temp. of deflection under load (1.80 MPa) 102 °C ISO 75-1/-2
Temp. of deflection under load (0.45 MPa) 106 °C ISO 75-1/-2
Vicat softening temperature, 50°C/h 50N 105 °C ISO 306
Burning behav. at 1.5 mm nom. thickn. HB class UL 94
Thickness tested 1.6 mm IEC 60695-11-10
Coeff. of linear therm. expansion, parallel 40 E-6/K ISO 11359-1/-2
Coeff. of linear therm. expansion, normal 80 E-6/K ISO 11359-1/-2

Electrical Properties Value Unit Test Standard


ISO Data
Relative permittivity, 100Hz 2.9 - IEC 60250
Relative permittivity, 1MHz 3.1 - IEC 60250
Dissipation factor, 100Hz 40 E-4 IEC 60250
Dissipation factor, 1MHz 60 E-4 IEC 60250
Volume resistivity >1E13 Ohm*m IEC 60093
Surface resistivity 1E14 Ohm IEC 60093
Electric strength 32 kV/mm IEC 60243-1
Comparative tracking index 575 - IEC 60112

Other Properties Value Unit Test Standard


ISO Data
Density 1160 kg/m³ ISO 1183

Rheological calculation properties Value Unit Test Standard


ISO Data
Density of melt 985 kg/m³ -
Thermal conductivity of melt 0.144 W/(m K) -
Spec. heat capacity of melt 1640 J/(kg K) -
Ejection temperature 95 °C -

Test specimen production Value Unit Test Standard


ISO Data
Injection Molding, melt temperature 240 °C ISO 294
Injection Molding, mold temperature 70 °C ISO 10724
Injection Molding, injection velocity 540 mm/s ISO 294

Created: 2015-08-04 Source: www.materialdatacenter.com Copyright M-Base Engineering+Software GmbH. Page: 1/2
Novodur® P2HGV
ABS-GF16 Styrolution

Diagrams

Viscosity-shear rate Shearstress-shear rate

Viscosity-shear rate Shearstress-shear rate


Novodur® P2HGV Novodur® P2HGV

1E4 220 °C 1E6 220 °C


240 °C 240 °C
260 °C 260 °C
280 °C 280 °C
1E3

Shearstress in Pa
Viscosity in Pa s

1E2 1E5

1E1

1E0 1E4
1E1 1E2 1E3 1E4 1E5 1E1 1E2 1E3 1E4 1E5

Shear rate in 1/s Shear rate in 1/s

Dynamic Shear modulus-temperature

Dynamic Shear modulus-temperature


Novodur® P2HGV

1E4 1E1
1E3 G'
G"
tan d
Shear modulus in MPa

1E3
1E2 1E0
G" in MPa

tan d

1E2 1E-1
1E1

1E1
1E0 1E-2

1E0 1E-3
1E-1-50 0 50 100 150

Temperature in °C

Characteristics

Processing Delivery form


Injection Molding Pellets

Disclaimer
These are guide values and not a specification. The guide values are measured and provided by the product manufacturer. M-Base has taken
the guide values from the producer's original Technical Data Sheet. Neither ALBIS nor M-Base is responsible / liable for the accuracy of the
guide values. Any information given on the chemical and physical characteristics of products supplied by ALBIS, including technical advice on
applications whether verbally, in writing or by testing the product, is given to the best of our knowledge. It does not exempt the buyer from
carrying out their own investigations and tests in order to ascertain the product's specific suitability for the purpose intended. The buyer is
solely responsible for the application, utilization and processing of the product, and must observe the laws and government regulations and the
consequential rights of third parties. ALBIS expressly advises against the use of this product in any medical, pharmaceutical or diagnostic
application. At all times our Conditions of Sale apply.

Created: 2015-08-04 Source: www.materialdatacenter.com Copyright M-Base Engineering+Software GmbH. Page: 2/2