You are on page 1of 1

REPORT OF FLAMMABILITY TEST RESULT

1. MATERIAL IDENTIFICATION
Material Grade : POM Plate

2. FLAMMABILITY TEST : MVSS302


Testing Place : PT MCNS Polyurethanes Indonesia, Cikampek
Testing Date : August 2nd 2017
Testing Foam Sample : POM plate Samples (5 pcs)
Size of specimen for testing 193-195x115-118x3mm (thickness)
Tested by : Fransiskus Meirawan

3. TEST RESULT
Burning Test
Name Burning Length Burning Time Burn Speed
Results
mm sec mm/min
1 Burn Bottom Plate 157 362 26.0 Burn
2 Burn Bottom Plate 155 365 25.5 Burn
3 Burn Bottom Plate 156 363 25.8 Burn
4 Burn Top Plate 156 387 24.2 Burn
5 Burn Top Plate 155 360 25.8 Burn

5 4 3 2 1

Remark : Sample length less than 330 mm. Burning time and length measure after pass A Line
4. CONCLUSION

According to MVSS302 Flammability result of POM plate samples were Burn

Tested By

Fransiskus Meirawan