You are on page 1of 2

MARSHALL TEST DATA

[As per ASTM D: 1559]


Source of Material : Plant
Type of Material : BC Material
Chainage / Location : Lab
Layer :BC Layer
Proposed Use :BC Design
Grade of Bitumen :CRMB-60
Proving Ring No. :
Correction Factor of Proving Ring : 7.137

%
% Agg Bulk Max.
Bitumen Wt of Wt of Wt of SSD
Content of Volume, Density Theoretica
Sl. No. Content of Sample in Sample in Sample in
Total Mix cc (Gmb), l Sp. Gr.
Total Mix Air, gm Water, gm Air, gm
(Ps) g/cc (Gmm)
(Pb)

1 2 3 4 5 6 7 8
1 5.00 95.0 1200.0 706.0 1209.0 503.0 2.386 2.697
2 5.00 95.0 1196.0 704.0 1204.0 500.0 2.392 2.697
3 5.00 95.0 1198.0 711.0 1212.0 501.0 2.391 2.697
Average 2.390 2.697
1 5.0 95.0 1199.0 703.0 1206.0 503.0 2.384 2.697
2 5.0 95.0 1201.0 705.0 1209.0 504.0 2.383 2.697
3 5.0 95.0 1196.0 704.0 1204.0 500.0 2.392 2.697
Average 2.386 2.697

Average of Both set 2.388 2.6966147

Remarks :
Density 2.388
GMM 2.697
Air Voids 11.45
VMA 21.96
VFB 47.88
ALL TEST DATA
ASTM D: 1559]
Date of Sampling
Date of Testing
Sampled by
Tested by
Bulk Specific Gravity (Gsb) 2.907
Effective Specific Gravity (Gse) 2.952
Apparent Specific Gravity (Gsa) 2.996
Specific Gravity of Bitumen (Gb) 1.02

% Air
Correction
Voids in Proving
% VMA = % VFB = Factor Corrected
Mix, Va = Ring Stability,
100- (10- (Based on Stability, Flow, mm
Reading, Kg
(7*2/Gsb) 9/ 10)*100 volume of Kg
100X(8- KN
specimen)
7)/8)
9 10 11 12 13 14 15 16
11.53 22.04 47.68 140 999.2 1.19 1189.0 3.8
11.30 21.83 48.25 150 1070.6 1.19 1274.0 4.5
11.33 21.86 48.18 130 927.8 1.19 1104.1 4.1
11.38 21.91 48.04 1189.0 4.1
11.60 22.10 47.50 135 963.5 1.19 1146.6 4.2
11.63 22.13 47.43 140 999.2 1.19 1189.0 4.6
11.30 21.83 48.25 130 927.8 1.19 1104.1 4.3
11.51 22.02 47.73 1146.6 4.4

11.45 21.96 47.88 1167.8 4.25