1 . Summary Trial Compaction


2 Skets lokasi dan Kepadatan lapangan
3 . Marshall Trial Compaction
4 . Marshall Index Retained Trial Compaction
5 . Marshall PRD Trial Compaction
6 . Gmm Trial Compaction
7 . Extraction Test
8.
9.
10 .
11 .
PROYEK SCRAPP AND FILL PERKERASAN JALAN TOL
PADA JALAN TOL TANGERANG MERAK
TAHUN 2020

SUMMARY TRIAL COMPACTION


AC - WEARING COURSE ( AC-WC )
5-Apr-16
I. Aggregate
Gradasi Gradation
Spesifikasi Remark
ASTM Sieve Combined Agg. Extraction
1" inch 25.4 mm 100.00 100.00 100 - 100
3/4" inch 19.1 mm 100.00 100.00 100 - 100
1/2" inch 12.7 mm 92.09 96.81 90 - 100
3/8" inch 9.52 mm 81.75 80.93 77 - 90
No. 4 4.76 mm 57.69 59.87 53 - 69
No. 8 2.38 mm 43.19 44.43 33 - 53
No. 16 1.18 mm 32.65 34.32 21 - 40
No. 30 0.59 mm 21.46 23.51 14 - 30
No. 50 0.279 mm 14.96 14.53 9 - 22
No. 100 0.149 mm 9.47 8.69 6 - 15
No. 200 0.074 mm 5.86 5.48 4 - 9

II. Marshall Test

No. Properties Unit Test Result Spesifikasi Remark

1 Asphalt Content % 5.78


2 Bulk Density gr/cc 2.252
3 Dust Portion Ratio % 0.842 0.6 ~ 1.2
4 Maximum Specific Gravity (Gmm) gr/cc 2.353
5 Void In Mix (VIM) % 4.36 3.0 - 5.0
6 Void Filled With Bitumen (VFB) % 75.82 > 65
7 Void in Mineral Aggregate (VMA) % 18.02 > 15
8 Stabilitas kg 1365 > 1000
9 Kelelehan (Flow) mm 3.45 2.0 - 4.0
10 VIM PRD Asphalt Content 5.80% % 2.62 > 2
11 Stabilitas Sisa Perendaman 24 jam % 91.09 > 90

III. Field Test Result

No. Properties Unit Test Result Spesifikasi Remark

#NAME? 18 Passing
1 Density Lapangan % Min. 98
#NAME? 20 Passing
2 Tack Coat gr/cc 0.215 0.15 ~ 0.35 CRS-1

III. Composition For 1 Ton Mixture


Weigth Materials
No Hot Bin % by Agg % by Mix Remark
For 1 Ton
1 Asphalt 5.8 5.8 58 kg

2 Hot Bin I 48.0 45.2 452 kg


3 Hot Bin II 24.0 22.6 226 kg
4 Hot Bin III 28.0 26.4 264 kg
TOTAL 105.8 100 1000 kg

Diperiksa Oleh Disetujui Oleh


Dibuat Oleh
Kontraktor Owner
PT. WIDYA SAPTA CONTRACTOR ASTRA INFRA SOLUTIONS ASTRA INFRA TOLL ROAD
PROYEK PEKERJAAN KONSTRUKSI PRESERVASI JALAN
ANJIR PASAR (BTS. PROV KALTENG) BATI-BATI - BTS
KOTA PELAIHARI - KP. ASAM-ASAM
TAHUN 2020-2022

TRIAL COMPACTION
Proyek : ANJIR PASAR ASAM-ASAM MYC
Type of Mixtures : LTBA-B Halus

I. SKETS LOKASI TRIAL

Panjang Trial Compaction Banjarmasin


75+040 74+875 74+711

14 PASSING 16 PASSING 18 PASSING

II.RENCANA PENGGELARAN
No Tebal Desain Gelar Tebal gembur Factor losse perkiraan Keterangan
1 3 cm 4,5 cm 14 Passing
2 3 cm 4,5 cm 50% 16 Passing
3 3 cm 4,5 cm 18 Passing

III.PEMADATAN
Alat yang Berat Alat ( Ton ) Temperatur Variasi I Variasi II Variasi III
No. Alat Keterangan
Digunakan Alat+Air Spesifikasi Pemadatan 14 Passing 16 Passing 18 Passing
Kosong
1 Tandem 8 8.50 8 140 o C 2 2 2 Breakdown
2 Tire Roller 10.5 12.5 10 125 o C 14 16 18 Intermedite
3 Tandem 8 8.50 8 110 o C 2 2 2 Finishing

IV. SKETS LOKASI TITIK CORE DRILL TRIAL COMPACTION


0+600 0+580 0+560 0+540

0+550 R
0+590 CL 0+570 CL
14 Passing 16 Passing 18 Passing
V. HASIL TEST PEMADATAN
No. Variasi of Thickness Density Degre of
Keterangan
Sample Compaction t1 t2 t3 Average In Air In Water Ssd Volume Density lap. Density Lab. Compaction
1 14 Passing 2.9 2.9 2.9 2.90 504.5 297.0 505.0 208.0 2.425 2.264 107.1
2 16 Passing 3.2 3.2 3.1 3.17 537.2 318.0 537.8 219.8 2.444 2.264 108.0
3 18 Passing 2.6 2.8 2.8 2.73 487.1 289.0 487.6 198.6 2.453 2.264 108.3

Tebal Design gelar gembur Factor losse Perkiraan Tebal Real Real losse
Keterangan
cm cm % ( cm ) cm %
3 4.5 50 2.90 1.60 55.2 14 Passing
3 4.5 50 3.17 1.33 42.1 16 Passing
3 4.5 50 2.73 1.77 64.6 18 Passing

VI. KESIMPULAN
Berdasarkan hasil Trial Compaction Campuran LTBA-B Halus yang dilaksanakan pada tanggal : 20 Agustus 2021
Pada proyek pekerjaan Konstruksi Preservasi Jalan Anjir Pasar (BTS. PROV. KALTENG) - BATI-BATI - BTS. KOTA PELAIHARI - KP. ASAM-ASAM
dengan Percobaan Pemadatan 2-14-2 Passing, ternyata sudah tercapai untuk memenuhi standar minimal 98% kepadatan.
Maka Pelaksanaan selanjutnya dilapangan mengacu pada Variasi 1 tersebut yaitu :
1 Pemadatan Alat berat minimal Lintasan Temperature Factor losse Keterangan
1 Breakdown Tandaem 8 ton 2 Passing 140 o C
2 Intermidite Tire Roller 10 ton 14 Passing 125 o C Tetap 50 %
3 Finishing Tandem 8 ton 2 Passing 105 Co

Dibuat Oleh Diperiksa Oleh Disetujui Oleh


Penyedia Jasa, Konsultan Supervisi, Binamarga

RAMDAN PRAMEDIS SETYA DWI MULIA SH, ST AHMAD RIZAL FERDANA, ST


Quality Control Mat. Lab/Technician Pengawas Lapangan
PROYEK SCRAPP AND FILL PERKERASAN JALAN TOL
PADA JALAN TOL TANGERANG MERAK
TAHUN 2020

COATING

Project : PROYEK SCRAPP AND FILL PERKERASAN JALAN TOL Date test : 25/09/2020 Paper Size : 25 x 25 cm
Description : AC-WEARING COURSE Test by : Ulfi Temperature : 60oC
g/cc
Location : Material : CRS- I Sp.Gravity : 1.015

WEIGHT (gram) Paper Size TOTAL BITUMEN


LOCATION LINE TEST
No. PAP + BIT PAPER BITUMEN 25 cm x 25 cm ( ltr / m2 ) REMARKS
POINT
FROM STA TO STA L/R a b c = a- b d e = ( c/d ) / 1000 /Sp.Gr.
1 75+150 74+919 L1 75+125 25 10.0 15 0.0625 0.24
2 L1 75+075 20 10.0 10 0.0625 0.16
3 L1 75+025 18 10.0 8 0.0625 0.13
4 L1 74+975 18 10.0 8 0.0625 0.13
5 L1 75+115 24 10.0 14 0.0625 0.22
6 L1 75+065 30 10 20 0.0625 0.32
7 L1 75+015 28 10 18 0.0625 0.28
8 L1 74+950 26 10 16 0.0625 0.25

AVERAGE 0.215

Diperiksa Oleh Disetujui Oleh


Dibuat Oleh
Kontraktor Owner
PT. WIDYA SAPTA CONTRACTOR ASTRA INFRA SOLUTIONS ASTRA INFRA TOLL ROAD
PROYEK SCRAPP AND FILL PERKERASAN JALAN TOL
PADA JALAN TOL TANGERANG MERAK
TAHUN 2020

MARSHALL STABILITY AND FLOW OF BITUMINOUS PAVING MIXTURES


ASTM D-6927
Penetration Grade AC 60 / 70 Date of Production : 25/9/2020
Sp. Gravity of Asphalt Gb 1.030 Project : SFO pada jalan Tol Merak
Bulk Sp. Gravity of Aggregates Gsb 2.586 Type of Mixtures : AC- WEARING COURSE
Effective Sp. Gravity of Aggregates Gse 2.648 Source of Materials : AMP WASCO
Bitumen Absorption Pba 0.924 Tested by : Johar
Number of Blows 75 Checked by : Roni
Calibration of Proving Ring 60.00 lbf Temperature of Mixtures : 152.0 o
C

WEIGHT OF SPECIMENS VOLUME SPECIFIC GRAVITY VOID PERCENTAGE STABILITY EFFECTIVE


Bitumen Bitumen
OF Void In Mineral Void In Void Filled BITUMEN Keterangan
Content Content Bulk Max. Theoritis/ Measurement Stability Adjusted FLOW CONTENT
In Air In Water SSD SPECIMENS Density By Vacuum Aggregates Mixtures with Bitumen Reading Correlation Stability
AC Pb Gmb Gmm VMA VIM VFB Ratio Pbe
Specimen
No. a b c d e f g h i j k l m n o p q

Total Total 100 (l x lbf x m)


Weight Weight e-d c (100-b) + b 100 - (100-b).g 100 - (100 g) 100 ( i - j ) x b - Pba (100-b)
by Agg. by Mix f Gse Gb Gsb h i 0.4536 100
% % gram gram gram cm3 gram/cm3 gram/cm3 % % % kg mm %

Marshall Test Trial Compaction


1 5.78 1151.6 645.1 1157.3 512.2 2.248 2.353 18.09 4.45 75.42 48.0 1.00 1306 3.30 4.914
2 5.78 1153.6 646.2 1159.2 513.0 2.249 2.353 18.08 4.43 75.49 51.0 1.00 1388 3.20 4.914
3 5.78 1150.8 648.2 1158.5 510.3 2.255 2.353 17.85 4.16 76.70 51.0 1.00 1388 3.60 4.914
4 5.78 1149.7 644.9 1156.4 511.5 2.248 2.353 18.12 4.48 75.30 51.0 1.00 1388 3.60 4.914
5 5.78 1151.4 646.7 1158.3 511.6 2.251 2.353 18.01 4.35 75.84 47.0 1.00 1279 3.70 4.914
6 5.78 1152.6 646.4 1158.1 511.7 2.252 2.353 17.94 4.27 76.19 53.0 1.00 1442 3.30 4.914
7 5.78 1147.2 646.8 1156.3 509.5 2.252 2.353 17.97 4.31 76.03 58.0 1.00 1579 3.30 4.914
8 5.78 1146.1 647.6 1156.2 508.6 2.253 2.353 17.91 4.23 76.37 55.0 1.04 1557 3.40 4.914
9 5.78 1150.1 646.4 1157.8 511.4 2.249 2.353 18.07 4.42 75.53 56.0 1.00 1524 3.20 4.914
10 5.78 1150.9 648.3 1158.7 510.4 2.255 2.353 17.85 4.17 76.65 48.0 1.00 1306 3.70 4.914
11 5.78 1151.7 647.7 1157.6 509.9 2.259 2.353 17.72 4.01 77.37 49.0 1.00 1334 3.30 4.914
12 5.78 1141.9 647.3 1153.6 506.3 2.255 2.353 17.84 4.15 76.74 51.0 1.04 1444 3.60 4.914
Rata - rata 2.252 2.353 18.02 4.36 75.82 1365 3.45 4.914
Spesifikasi > 15 3-5 > 65 > 1000 2~4

Diperiksa Oleh Disetujui Oleh


Dibuat Oleh
Kontraktor Owner
PT. WIDYA SAPTA CONTRACTOR ASTRA INFRA SOLUTIONS ASTRA INFRA TOLL ROAD
PROYEK SCRAPP AND FILL PERKERASAN JALAN TOL
PADA JALAN TOL TANGERANG MERAK
TAHUN 2020

MARSHALL STABILITY AND FLOW OF BITUMINOUS PAVING MIXTURES


ASTM D-6927

Penetration Grade AC 60 / 70 Date of Production : 25-09-2020


Sp. Gravity of Asphalt Gb 1.030 Project : SFO Jalan Tol Merak
Bulk Sp. Gravity of Aggregates Gsb 2.586 Type of Mixtures : AC - WEARING COURSE
Effective Sp. Gravity of Aggregates Gse 2.648 Source of Materials : AMP WASCO
Bitumen Absorption Pba 0.924 Tested by : Johar
Number of Blows 75 Checked by : Roni
Calibration of Proving Ring 60.00 lbf Temperature of Mixtures : 152.0 o
C

WEIGHT OF SPECIMENS SPECIFIC GRAVITY VOID PERCENTAGE STABILITY


Bitumen Bitumen VOLUME EFFECTIVE Keterangan
Content Content OF Bulk Max. Theoritis/VOID PERCENTAGE Void In Void Filled Measurement Stability Adjusted FLOW BITUMEN
In Air In Water SSD SPECIMENS Density By Vacuum Aggregates Mixtures with Bitumen Reading Correlation Stability CONTENT
Specimen AC Pb Gmb Gmm VMA VIM VFB Ratio
No. a b c d e f g h i j k l m n o q q
Total Total 100 (l x lbf x m)
Weight Weight e-d c (100-b) + b 100 - (100-b).g 100 - (100 g) 100 ( i - j ) x b - Pba (100-b)
by Agg. by Mix f Gse Gb Gsb h i 0.4536 100
% % gram gram gram cm3 gram/cm3 gram/cm3 % % % kg mm %

Marshall Test Trial Compaction


1 5.78 1151.6 645.1 1157.3 512.2 2.248 2.353 18.09 4.45 75.42 48.0 1.00 1306 3.30 4.914
2 5.78 1153.6 646.2 1159.2 513.0 2.249 2.353 18.08 4.43 75.49 51.0 1.00 1388 3.20 4.914
3 5.78 1150.8 648.2 1158.5 510.3 2.255 2.353 17.85 4.16 76.70 51.0 1.00 1388 3.60 4.914
4 5.78 1149.7 644.9 1156.4 511.5 2.248 2.353 18.12 4.48 75.30 51.0 1.00 1388 3.60 4.914
5 5.78 1151.4 646.7 1158.3 511.6 2.251 2.353 18.01 4.35 75.84 47.0 1.00 1279 3.70 4.914
6 5.78 1152.6 646.4 1158.1 511.7 2.252 2.353 17.94 4.27 76.19 53.0 1.00 1442 3.30 4.914
7 5.78 1147.2 646.8 1156.3 509.5 2.252 2.353 17.97 4.31 76.03 58.0 1.00 1579 3.30 4.914
8 5.78 1146.1 647.6 1156.2 508.6 2.253 2.353 17.91 4.23 76.37 55.0 1.04 1557 3.40 4.914
9 5.78 1150.1 646.4 1157.8 511.4 2.249 2.353 18.07 4.42 75.53 56.0 1.00 1524 3.20 4.914
10 5.78 1150.9 648.3 1158.7 510.4 2.255 2.353 17.85 4.17 76.65 48.0 1.00 1306 3.70 4.914
11 5.78 1151.7 647.7 1157.6 509.9 2.259 2.353 17.72 4.01 77.37 49.0 1.00 1334 3.30 4.914
12 5.78 1141.9 647.3 1153.6 506.3 2.255 2.353 17.84 4.15 76.74 51.0 1.04 1444 3.60 4.914
Average 1149.8 646.8 1151.6 510.5 2.252 2.353 17.95 4.29 76.14 1411 3.43 4.914

Marshall Test Trial Mix Index Retained Soaked 24 hour


1 5.78 1155.2 648.6 1161.6 513.0 2.252 2.353 17.97 4.30 76.07 45.0 1.09 1335 3.70 4.914
2 5.78 1154.9 646.8 1159.8 513.0 2.251 2.353 17.99 4.32 75.96 44.0 1.09 1305 3.80 4.914
3 5.78 1149.7 643.2 1154.3 511.1 2.249 2.353 18.05 4.40 75.63 41.0 1.09 1216 3.60 4.914
Average 1153.3 646.2 1158.6 512.4 2.251 2.353 18.00 4.34 75.89 1286 3.70 4.914

1286
Stability Index Retained Marshall Trial Mix 5.5% Soaked in Water 60 oC for 24 hour = x 100% = 91.09
1411
Spesifikasi > 90

Diperiksa Oleh Disetujui Oleh


Dibuat Oleh
Kontraktor Owner
PT. WIDYA SAPTA CONTRACTOR ASTRA INFRA SOLUTIONS ASTRA INFRA TOLL ROAD
PROYEK SCRAPP AND FILL PERKERASAN JALAN TOL
PADA JALAN TOL TANGERANG MERAK
TAHUN 2020

MARSHALL STABILITY AND FLOW OF BITUMINOUS PAVING MIXTURES


ASTM D-6927
Penetration Grade AC 60 / 70 Date of Production : 26-09-2020
Sp. Gravity of Asphalt Gb 1.030 Project : SFO Jalan Tol Merak
Bulk Sp. Gravity of Aggregates Gsb 2.586 Type of Mixtures : AC - WEARING COURSE
Effective Sp. Gravity of Aggregates Gse 2.648 Source of Materials : AMP WASCO
Bitumen Absorption Pba 0.924 Tested by : Johar
Number of Blows 400 Checked by : Roni
Calibration of Proving Ring 60.00 lbf Temperature of Mixtures : 150.0 o
C

WEIGHT OF SPECIMENS SPECIFIC GRAVITY VOID PERCENTAGE STABILITY EFFECTIVE


Bitumen Bitumen VOLUME
OF Void In Mineral Void In Void Filled BITUMEN
Content Content Bulk Max. Theoritis/ Measurement Stability Adjusted FLOW CONTENT
In Air In Water SSD SPECIMENS Density By Vacuum Aggregates Mixtures with Bitumen Reading Correlation Stability
AC Pb Gmb Gmm VMA VIM VFB Ratio Pbe
Specimen
No. a b c d e f g h i j k l m n o q q

Total Total 100 (l x lbf x m)


Weight Weight e-d c (100-b) + b 100 - (100-b).g 100 - (100 g) 100 ( i - j ) x b - Pba (100-b)
by Agg. by Mix f Gse Gb Gsb h i 0.4536 100
% % gram gram gram cm3 gram/cm3 gram/cm3 % % % kg mm %

Marshall Percentage Refusal Density (PRD)


### 1 5.78 1154.2 653.5 1156.1 502.6 2.296 2.357 16.34 2.57 84.30 25.0 1.04 708 3.70 191 4.914
### 2 5.78 1151.6 651.9 1153.3 501.4 2.297 2.357 16.33 2.55 84.37 28.0 1.04 793 4.20 189 4.914
### 3 5.78 1153.6 652.4 1155.7 503.3 2.292 2.357 16.50 2.75 83.32 27.5 1.04 778 3.90 200 4.914
Average 1153.13 652.60 1155.03 502.43 2.295 2.357 16.39 2.62 84.00
Spesifikasi >15 >2 >65

Diperiksa Oleh Disetujui Oleh


Dibuat Oleh
Kontraktor Owner
PT. WIDYA SAPTA CONTRACTOR ASTRA INFRA SOLUTIONS ASTRA INFRA TOLL ROAD

1224.1 684.1 1235.2 551.1 2.221


1225.9 685.7 1238.1 552.4 2.219
1213.0 677.9 1223.8 545.9 2.222
1221.0 682.6 1232.4 549.8 2.221
1221.4 683.6 1231.0 547.4 2.231
1229.3 687.5 1237.2 549.7 2.236
1221.8 684.1 1232.2 548.1 2.229
1224.2 685.1 1233.5 548.4 2.232
1228.8 687.2 1234.9 547.7 2.244
1225.5 686.4 1231.2 544.8 2.249
1260.5 706.6 1267.4 560.8 2.248
1238.3 693.4 1244.5 551.1 2.247
1226.5 688.9 1231.4 542.5 2.261
1223.9 686.4 1229.0 542.6 2.256
1216.0 683.2 1220.7 537.5 2.262
1222.1 686.2 1227.0 540.9 2.260
1214.1 680.9 1219.3 538.4 2.255
1214.5 681.7 1218.9 537.2 2.261
1211.8 679.1 1215.9 536.8 2.257
1213.5 680.6 1218.0 537.5 2.258
28.9 0.89 1128 3.20 352
27.6 0.89 1077 3.80 283
30.8 0.93 1256 3.20 393

1410 3.23 437


PROYEK SCRAPP AND FILL PERKERASAN JALAN TOL
PADA JALAN TOL TANGERANG MERAK
TAHUN 2020

BERAT JENIS CAMPURAN MAKSIMUM


(Gmm)

ASTM D-2041
Pekerjaan / Proyek : PROYEK SCRAPP AND FILL PERKERASAN JALAN TOL Tanggal : 25/9/2020
Sumber Material : AMP WASCO Dikerjakan : Johar
Jenis Campuran : AC WEARING COURSE Diperiksa : Roni

NOMOR BENDA UJI 1 2 3 4 5

Unit Keterangan
5.8 5.50 6.00
Asphalt Content
% % %

1. Berat Pycnometer + Contoh g 4958.6 4112.5 4103.7

2. Berat Pycnometer + Lid g 2984.0 2988.0 2988.0

3. Berat Contoh 1-2 g 1974.6 1124.5 1115.7

4. Berat Pycnometer + A i r g 7467.0 7477.8 7477.8

5. Berat Pycnometer + Air + Contoh g 8602.5 8127.5 8119.6

6. Berat Jenis 3 / ( 3 + 4 -5 ) g/cm3 2.353 2.368 2.354

7. Temperature Air o
C 25.5 26.0 25.5

8. Faktor Koreksi Temperature 0.9999 0.9997 0.9999


9. Berat Jenis Terkoreksi 6x8 g/cm3 2.353 2.368 2.354

Remarks :

Diperiksa Oleh Disetujui Oleh


Dibuat Oleh
Kontraktor Owner
PT. WIDYA SAPTA CONTRACTOR ASTRA INFRA SOLUTIONS ASTRA INFRA TOLL ROAD
PROYEK SCRAPP AND FILL PERKERASAN JALAN TOL
PADA JALAN TOL TANGERANG MERAK
TAHUN 2020

QUANTITATIVE EXTRACTION OF BITUMEN


FROM BITUMINOUS PAVING MIXTURES
TRIAL COMPACTION
ASTM D-2172
Pekerjaan / Proyek : PROYEK SCRAPP AND FILL PERKERASAN JALAN TOL Sample : Lab. Crew Tanggal : 25/9/2020
Sumber Material : AMP WASCO Dikerjakan : Johar Tanggal : 25/9/2020
Jenis Campuran : AC WEARING COURSE Diperiksa : Roni Tanggal : 25/9/2020

Weight of Sample Weight of Filter Weight Weight of Weight of Bitumen


Sample before after before after of Filler Total Agg. Bitumen Content
Remarks
No. a b c d e=d-c f=b+e g=a-f h = g/a x 100
gram gram gram gram gram gram gram %
1 1087.3 1018.5 13.5 19.4 5.9 1024.4 62.9 5.78

AVERAGE 5.78

Sample No 1 2 Average

ASTM SPECIFICATION
Weight Accum. Percent Percent Weight Accum. Percent Percent Percent
Sieve LIMIT
Retained Retained Retained Passing Retained Retained Retained Passing Passing
Size
inch mm gram gram % % gram gram % % %
1" 25.4 0.0 0.00 100.00 100 - 100
3/4" 19.0 0.0 0.00 100.00 100 - 100
1/2" 12.7 32.7 3.19 96.81 90 - 100
3/8" 9.50 195.4 19.07 80.93 77 - 90
No. 4 4.75 411.1 40.13 59.87 53 - 69
No. 8 2.36 569.3 55.57 44.43 33 - 53
No. 16 1.18 672.8 65.68 34.32 21 - 40
No. 30 0.59 783.6 76.49 23.51 14 - 30
No. 50 0.279 875.6 85.47 14.53 9 - 22
No. 100 0.149 935.4 91.31 8.69 6 - 15
No. 200 0.075 968.3 94.52 5.48 4 - 9
PAN 1024.4

EXTRACTION TEST
100
90
PASSING PERCENTAGE ( % )

80
70 SPESIFIKASI MAX.

60
50
EXTRACTION TEST
40 AGGREGATE GRADATION
30 SPESIFIKASI MIN.

20
10
0
0.0No. 200 No. 100 No.0.1
50 No. 30 No. 161.0 No. 8 No. 4 10.0 3/8" 1/2" 3/4" 1" 100.0
SIEVE SIZE

Diperiksa Oleh Disetujui Oleh


Dibuat Oleh
Kontraktor Owner
PT. WIDYA SAPTA CONTRACTOR ASTRA INFRA SOLUTIONS ASTRA INFRA TOLL ROAD
0 Doc No : WSC.IV.q/PRJ-060
PROYEK SCRAPP AND FILL PERKERASAN JALAN TOL Rev No :0
PADA JALAN TOL TANGERANG MERAK Rev Date :0

MARSHALL STABILITY AND FLOW OF BITUMINOUS PAVING MIXTURES


ASTM D-6927
Penetration Grade AC 60 / 70 Date of Production : 17/06/2015
Sp. Gravity of Asphalt Gb 1.030 Project : Peningkatan Jalan Cilodong/Batas Depok
Bulk Sp. Gravity of Aggregates Gsb #REF! Type of Mixtures : AC - Wearing Course
Effective Sp. Gravity of Aggregates Gse #REF! #REF! Source of Materials : AMP Cakung - Jakarta
Bitumen Absorption Pba #REF! #REF! Tested by : Handita, Ulfi
Number of Blows 75 Checked by : T. Hidayat
Calibration of Proving Ring 42.06 lbf Temperature of Mixtures : 151.2 o
C

WEIGHT OF SPECIMENS VOLUME SPECIFIC GRAVITY VOID PERCENTAGE STABILITY EFFECTIVE


Bitumen Bitumen
OF Void In Mineral Void In Void Filled MARSHALL BITUMEN
Content Content Bulk Max. Theoritis/ Measurement Stability Adjusted FLOW
QUOTIENT CONTENT
In Air In Water SSD SPECIMENS Density By Vacuum Aggregates Mixtures with Bitumen Reading Correlation Stability
AC Pb Gmb Gmm VMA VIM VFB Ratio Pbe
Specimen
No. a b c d e f g h i j k l m n o p q

Total Total 100 (l x lbf x m)


Weight Weight e-d c (100-b) + b 100 - (100-b).g 100 - (100 g) 100 ( i - j ) x n b - Pba (100-b)
by Agg. by Mix f Gse Gb Gsb h i 0.4536 o 100
% % gram gram gram cm3 gram/cm3 gram/cm3 % % % kg mm kg/mm %

Marshall Test Trial Mix Batch Asphalt Content 5.80%


1 5.80 5.80 1204.29 680.26 1206.10 525.84 2.290 Err:509 #REF! Err:509 #REF! 85.0 0.96 1557 2.70 577 #REF!
2 5.80 5.80 1204.97 682.52 1205.95 523.43 2.302 Err:509 #REF! Err:509 #REF! 95.0 0.96 1740 2.60 669 #REF!
3 5.80 5.80 1203.74 684.82 1204.68 519.86 2.316 Err:509 #REF! Err:509 #REF! 97.0 1.00 1851 2.50 740 #REF!
4 4.50 5.80 1202.53 680.91 1203.86 522.95 2.300 Err:509 #REF! Err:509 #REF! 93.0 1.00 1774 2.50 710 #REF!
5 4.50 5.80 1203.47 682.53 1204.80 522.27 2.304 Err:509 #REF! Err:509 #REF! 85.0 1.00 1622 2.10 772 #REF!
6 4.50 5.80 1203.61 683.54 1204.40 520.86 2.311 Err:509 #REF! Err:509 #REF! 92.0 1.00 1755 2.50 702 #REF!
7 5.00 5.80 1200.14 680.25 1202.06 521.81 2.300 Err:509 #REF! Err:509 #REF! 90.5 1.00 1727 2.85 606 #REF!
8 5.00 5.80 1202.63 681.47 1204.11 522.64 2.301 Err:509 #REF! Err:509 #REF! 86.0 1.00 1641 2.70 608 #REF!
9 5.00 5.80 1195.78 676.35 1197.30 520.95 2.295 Err:509 #REF! Err:509 #REF! 92.5 1.00 1765 2.85 619 #REF!
10 5.50 5.80 1204.09 683.66 1205.45 521.79 2.308 Err:509 #REF! Err:509 #REF! 95.0 1.00 1812 2.90 625 #REF!
11 5.50 5.80 1198.17 678.90 1200.27 521.37 2.298 Err:509 #REF! Err:509 #REF! 91.5 1.00 1746 2.50 698 #REF!
12 5.50 5.80 1203.25 680.38 1205.09 524.71 2.293 Err:509 #REF! Err:509 #REF! 87.0 1.00 1660 2.70 615 #REF!

Average 1202.22 681.30 1203.67 522.37 2.301 Err:509 #REF! Err:509 #REF! 1721 2.62 662 #REF!

Diajukan Oleh Diperiksa Oleh Disetujui Oleh


Err:509 Err:509 Err:509
0
PROYEK SCRAPP AND FILL PERKERASAN JALAN TOL
PADA JALAN TOL TANGERANG MERAK

DETERMINATION VOID IN MIXTURE


V I M 7%

Pekerjaan / Proyek : #REF! Tanggal : #REF!


Sumber Material : #REF! Dikerjakan : Handita, Yani
Jenis Campuran : #REF! Diperiksa : #REF!

NOMOR BENDA UJI 1 2 3 4 5

Asphalt Content Unit #REF! #REF! #REF! #REF! #REF! Remarks

No. Of Blows 2 x 40 2 x 50 2 x 60 2 x 75

Maximum Specific Gravity of Mixture


A gr/cc Err:509 Err:509 Err:509 Err:509
(Gmm)

Average of Bulk Density B gr/cc 2.186 2.218 2.242 2.263

A-B
VIM = x 100 C gr/cc Err:509 Err:509 Err:509 Err:509
A
40 50 60 75
Err:509 Err:509 Err:509 Err:509

BLOWS >< VIM


8.00

7.00
VOID IN MIXTURE (%)

6.00

5.00

4.00

3.00

2.00
35 40 45 50 55 60 65 70 75 80
NO. OF BLOWS

DETERMINATION VOID IN MIXTURE (VIM) 7% 41 Blows

Diajukan Oleh Diperiksa Oleh Disetujui Oleh


Err:509 Err:509 Err:509
0 Doc No : WSC.IV.q/PRJ-060
PROYEK SCRAPP AND FILL PERKERASAN JALAN TOL Rev No :0
PADA JALAN TOL TANGERANG MERAK Rev Date :0

MARSHALL STABILITY AND FLOW OF BITUMINOUS PAVING MIXTURES


ASTM D-6927
Penetration Grade AC 60 / 70 Date of Production : #REF!
Sp. Gravity of Asphalt Gb 1.030 Project : #REF!
Bulk Sp. Gravity of Aggregates Gsb #REF! Type of Mixtures : #REF!
Effective Sp. Gravity of Aggregates Gse #REF! #REF! Source of Materials : #REF!
Bitumen Absorption Pba #REF! #REF! Tested by : Handita
Number of Blows #REF! Checked by : #REF!
Calibration of Proving Ring #REF! lbf Temperature of Mixtures : 152.0 C
o

WEIGHT OF SPECIMENS SPECIFIC GRAVITY VOID PERCENTAGE STABILITY EFFECTIVE


Bitumen Bitumen VOLUME
OF Void In Mineral Void In Void Filled MARSHALL BITUMEN
Content Content Bulk Max. Theoritis/ Measurement Stability Adjusted FLOW
QUOTIENT CONTENT
In Air In Water SSD SPECIMENS Density By Vacuum Aggregates Mixtures with Bitumen Reading Correlation Stability
AC Pb Gmb Gmm VMA VIM VFB Ratio Pbe
Specimen
No. a b c d e f g h i j k l m n o p q

Total Total 100 (l x lbf x m)


Weight Weight e-d c (100-b) + b 100 - (100-b).g 100 - (100 g) 100 ( i - j ) x n b - Pba (100-b)
by Agg. by Mix f Gse Gb Gsb h i 0.4536 o 100
% % gram gram gram cm3 gram/cm3 gram/cm3 % % % kg mm kg/mm %

Marshall Asphalt Content 5.80% 2 x 75 Blows


1 5.80 5.80 1200.51 674.49 1204.79 530.30 2.264 Err:509 #REF! Err:509 #REF! 72.5 0.96 #REF! 3.15 #REF! #REF!
2 5.80 5.80 1198.66 673.91 1203.06 529.15 2.265 Err:509 #REF! Err:509 #REF! 71.0 0.96 #REF! 2.90 #REF! #REF!
3 5.80 5.80 1203.08 675.62 1208.14 532.52 2.259 Err:509 #REF! Err:509 #REF! 65.2 0.96 #REF! 3.10 #REF! #REF!
Average 1200.75 674.67 1205.33 530.66 2.263 Err:509 #REF! Err:509 #REF! #REF! 3.05 #REF! #REF!

Marshall Asphalt Content 5.80% 2 x 60 Blows


1 5.80 5.80 1199.60 670.95 1204.95 534.00 2.246 Err:509 #REF! Err:509 #REF! 65.8 0.96 #REF! 3.70 #REF! #REF!
2 5.80 5.80 1206.17 674.10 1211.26 537.16 2.245 Err:509 #REF! Err:509 #REF! 67.0 0.93 #REF! 3.50 #REF! #REF!
3 5.80 5.80 1197.33 667.15 1202.87 535.72 2.235 Err:509 #REF! Err:509 #REF! 64.5 0.93 #REF! 3.90 #REF! #REF!
Average 1201.03 670.73 1206.36 535.63 2.242 Err:509 #REF! Err:509 #REF! #REF! 3.70 #REF! #REF!

Marshall Asphalt Content 5.80% 2 x 50 Blows


1 5.80 5.80 1206.11 671.15 1213.16 542.01 2.225 Err:509 #REF! Err:509 #REF! 63.5 0.93 #REF! 3.70 #REF! #REF!
2 5.80 5.80 1200.45 661.94 1207.75 545.81 2.199 Err:509 #REF! Err:509 #REF! 61.0 0.93 #REF! 4.00 #REF! #REF!
3 5.80 5.80 1210.26 673.21 1216.40 543.19 2.228 Err:509 #REF! Err:509 #REF! 62.4 0.93 #REF! 3.80 #REF! #REF!
Average 1205.61 668.77 1212.44 543.67 2.218 Err:509 #REF! Err:509 #REF! #REF! 3.83 #REF! #REF!

Marshall Asphalt Content 5.80% 2 x 40 Blows


1 5.80 5.80 1207.81 662.75 1215.09 552.34 2.187 Err:509 #REF! Err:509 #REF! 58.2 0.89 #REF! 4.10 #REF! #REF!
2 5.80 5.80 1201.33 658.77 1209.44 550.67 2.182 Err:509 #REF! Err:509 #REF! 56.0 0.89 #REF! 3.90 #REF! #REF!
3 5.80 5.80 1205.47 662.55 1212.93 550.38 2.190 Err:509 #REF! Err:509 #REF! 60.0 0.89 #REF! 3.85 #REF! #REF!
Average 1204.87 661.36 1212.49 551.13 2.186 Err:509 #REF! Err:509 #REF! #REF! 3.95 #REF! #REF!

Diajukan Oleh Diperiksa Oleh Disetujui Oleh


Err:509 Err:509 Err:509
0.020 #REF!
0.025 #REF!
0.031 #REF!
0 Doc No : WSC.IV.q/PRJ-060
PROYEK SCRAPP AND FILL PERKERASAN JALAN TOL Rev No :0
PADA JALAN TOL TANGERANG MERAK Rev Date :0

MARSHALL STABILITY AND FLOW OF BITUMINOUS PAVING MIXTURES


ASTM D-6927
Penetration Grade AC 60 / 70 Date of Production : 27/04/2015
Sp. Gravity of Asphalt Gb 1.030 Project : #REF!
Bulk Sp. Gravity of Aggregates Gsb #REF! Type of Mixtures : #REF!
Effective Sp. Gravity of Aggregates Gse #REF! Source of Materials : #REF!
Bitumen Absorption Pba #REF! #REF! Tested by : Handita
Number of Blows #REF! Checked by : #REF!
Calibration of Proving Ring #REF! lbf Temperature of Mixtures : 151.0 o
C

WEIGHT OF SPECIMENS VOLUME SPECIFIC GRAVITY VOID PERCENTAGE STABILITY EFFECTIVE


Bitumen Bitumen
OF Void In Mineral Void In Void Filled MARSHALL BITUMEN
Content Content Bulk Max. Theoritis/ Measurement Stability Adjusted FLOW
QUOTIENT CONTENT
In Air In Water SSD SPECIMENS Density By Vacuum Aggregates Mixtures with Bitumen Reading Correlation Stability
AC Pb Gmb Gmm VMA VIM VFB Ratio Pbe
Specimen
No. a b c d e f g h i j k l m n o p q

Total Total 100 (l x lbf x m)


Weight Weight e-d c (100-b) + b 100 - (100-b).g 100 - (100 g) 100 ( i - j ) x n b - Pba (100-b)
by Agg. by Mix f Gse Gb Gsb h i 0.4536 o 100
% % gram gram gram cm3 gram/cm3 gram/cm3 % % % kg mm kg/mm %

Marshall Test Trial Mix Asphalt Content 5.80% 41 Blows for VIM 7%
1 5.80 5.80 1203.66 667.80 1211.83 544.03 2.212 Err:509 #REF! Err:509 #REF! 27.6 0.93 #REF! 3.90 #REF! #REF!
2 5.80 5.80 1201.45 656.80 1209.27 552.47 2.175 Err:509 #REF! Err:509 #REF! 26.5 0.93 #REF! 4.10 #REF! #REF!
3 5.80 5.80 1204.81 665.60 1212.10 546.50 2.205 Err:509 #REF! Err:509 #REF! 29.0 0.93 #REF! 3.70 #REF! #REF!
Average 1203.31 663.40 1211.07 547.67 2.197 Err:509 #REF! Err:509 #REF! #REF! 3.90 #REF! #REF!

Marshall Test Trial Mix Index Retained Asphalt Content 5.80% 41 Blows for VIM 7%
1 5.80 5.80 1198.35 674.00 1207.51 533.51 2.246 Err:509 #REF! Err:509 #REF! 23.5 0.89 #REF! 3.60 #REF! #REF!
2 5.80 5.80 1202.17 670.50 1210.04 539.54 2.228 Err:509 #REF! Err:509 #REF! 26.0 0.93 #REF! 4.00 #REF! #REF!
3 5.80 5.80 1201.44 669.20 1209.49 540.29 2.224 Err:509 #REF! Err:509 #REF! 26.5 0.89 #REF! 3.90 #REF! #REF!
Average 1200.65 671.23 1209.01 537.78 2.233 Err:509 #REF! Err:509 #REF! #REF! 3.83 #REF! #REF!

#REF!
Stability Index Retained Asphalt Content 5.80% Soaked in Water 60 oC for 24 hour = #REF! x 100% = #REF! %

Diajukan Oleh Diperiksa Oleh Disetujui Oleh


Err:509 Err:509 Err:509
0 Doc No : WSC.IV.q/PRJ-060
PROYEK SCRAPP AND FILL PERKERASAN JALAN TOL Rev No :0
PADA JALAN TOL TANGERANG MERAK Rev Date :0

MARSHALL STABILITY AND FLOW OF BITUMINOUS PAVING MIXTURES


ASTM D-6927
Penetration Grade AC 60 / 70 Date of Production : 18/06/2015
Sp. Gravity of Asphalt Gb 1.030 Project : #REF!
Bulk Sp. Gravity of Aggregates Gsb #REF! Type of Mixtures : #REF!
Effective Sp. Gravity of Aggregates Gse #REF! #REF! Source of Materials : #REF!
Bitumen Absorption Pba #REF! #REF! Tested by : Handita
Number of Blows #REF! Checked by : #REF!
Calibration of Proving Ring #REF! lbf Temperature of Mixtures : 151.0 o
C

WEIGHT OF SPECIMENS VOLUME SPECIFIC GRAVITY VOID PERCENTAGE STABILITY EFFECTIVE


Bitumen Bitumen
OF Void In Mineral Void In Void Filled MARSHALL BITUMEN
Content Content Bulk Max. Theoritis/ Measurement Stability Adjusted FLOW
QUOTIENT CONTENT
In Air In Water SSD SPECIMENS Density By Vacuum Aggregates Mixtures with Bitumen Reading Correlation Stability
AC Pb Gmb Gmm VMA VIM VFB Ratio Pbe
Specimen
No. a b c d e f g h i j k l m n o p q

Total Total 100 (l x lbf x m)


Weight Weight e-d c (100-b) + b 100 - (100-b).g 100 - (100 g) 100 ( i - j ) x n b - Pba (100-b)
by Agg. by Mix f Gse Gb Gsb h i 0.4536 o 100
% % gram gram gram cm3 gram/cm3 gram/cm3 % % % kg mm kg/mm %

Marshall Percentage Refusal Density (PRD) Asphalt Content 5.80% 2 x 400 Blows
1 5.80 5.80 1203.56 682.10 1207.31 525.21 2.292 Err:509 #REF! Err:509 #REF! 25.0 1.04 #REF! 3.70 #REF! #REF!
2 5.80 5.80 1200.48 678.92 1204.59 525.67 2.284 Err:509 #REF! Err:509 #REF! 28.0 1.04 #REF! 4.20 #REF! #REF!
3 5.80 5.80 1201.73 679.15 1205.17 526.02 2.285 Err:509 #REF! Err:509 #REF! 27.5 1.04 #REF! 3.90 #REF! #REF!

Average 1201.92 680.06 1205.69 525.63 2.287 Err:509 #REF! Err:509 #REF! #REF! 3.93 #REF! #REF!

Diajukan Oleh Diperiksa Oleh Disetujui Oleh


Err:509 Err:509 Err:509
Pekerjaan / Proyek : Pelebaran Ruas Kapuk - Pluit / Tol CTCSample : Lab. Crew Tanggal : 25/04/2015
Jenis Material : Hot Bin I / Trial Mix Batch Dikerjakan : Handita Tanggal : 25/04/2015
Sumber Material : AMP Cakung - Jakarta Diperiksa : T. Hidayat Tanggal : 25/04/2015

TEST 1 TEST 2
ASTM Berat Berat Average
KUMULATIF KUMULATIF
SIEVE tertahan tertahan Prosentase
SIZE Masing 2 Berat Prosentase Prosentase Masing 2 Berat Prosentase Prosentase Lolos Keterangan
Saringan Tertahan Tertahan Lolos Saringan Tertahan Tertahan Lolos
mm inch gram gram % % gram gram % % %
50.0 2" 0.00 0.00 0.00 100.00 0.00 0.00 0.00 100.00 100.00
37.5 1 1/2" 0.00 0.00 0.00 100.00 0.00 0.00 0.00 100.00 100.00
25.4 1" 0.00 0.00 0.00 100.00 0.00 0.00 0.00 100.00 100.00 100.00
19.1 3/4" 0.00 0.00 0.00 100.00 0.00 0.00 0.00 100.00 100.00 100.00
12.7 1/2" 0.00 0.00 0.00 100.00 0.00 0.00 0.00 100.00 100.00 100.00
9.5 3/8" 0.00 0.00 0.00 100.00 0.00 0.00 0.00 100.00 100.00 100.00
4.76 No. 4 0.00 0.00 0.00 100.00 0.00 0.00 0.00 100.00 100.00 99.47
2.38 No. 8 229.74 229.74 18.85 81.15 190.16 190.16 14.89 85.11 83.13 71.89
1.19 No. 16 338.44 568.18 46.62 53.38 380.92 571.08 44.72 55.28 54.33 51.27
0.59 No. 30 220.29 788.47 64.69 35.31 220.27 791.35 61.97 38.03 36.67 40.91
0.279 No. 50 97.15 885.62 72.66 27.34 113.92 905.27 70.89 29.11 28.23 31.83
0.149 No. 100 129.28 1014.90 83.27 16.73 134.92 1040.19 81.45 18.55 17.64 22.14
0.074 No. 200 81.10 1096.00 89.92 10.08 57.66 1097.85 85.97 14.03 12.06 11.03
Pan
BERAT CONTOH 1218.85 Gram 1277.06 Gram

Pekerjaan / Proyek : Pelebaran Ruas Kapuk - Pluit / Tol CTCSample : Lab. Crew Tanggal : 25/04/2015
Jenis Material : Hot Bin II / Trial Mix Batch Dikerjakan : T. Hidayat Tanggal : 25/04/2015
Sumber Material : AMP Cakung - Jakarta Diperiksa : T. Hidayat Tanggal : 25/04/2015

TEST 1 TEST 2
ASTM Berat Berat Average
KUMULATIF KUMULATIF
SIEVE tertahan tertahan Prosentase
SIZE Masing 2 Berat Prosentase Prosentase Masing 2 Berat Prosentase Prosentase Lolos Keterangan
Saringan Tertahan Tertahan Lolos Saringan Tertahan Tertahan Lolos
mm inch gram gram % % gram gram % % %
50.0 2" 0.00 0.00 0.00 100.00 0.00 0.00 0.00 100.00 100.00
37.5 1 1/2" 0.00 0.00 0.00 100.00 0.00 0.00 0.00 100.00 100.00
25.4 1" 0.00 0.00 0.00 100.00 0.00 0.00 0.00 100.00 100.00 100.00
19.1 3/4" 0.00 0.00 0.00 100.00 0.00 0.00 0.00 100.00 100.00 100.00
12.7 1/2" 0.00 0.00 0.00 100.00 0.00 0.00 0.00 100.00 100.00 100.00
9.5 3/8" 163.18 163.18 10.85 89.15 110.29 110.29 7.41 92.59 90.87 100.00
4.76 No. 4 891.74 1054.92 70.13 29.87 898.14 1008.43 67.76 32.24 31.05 99.47
2.38 No. 8 353.84 1408.76 93.66 6.34 360.34 1368.77 91.97 8.03 7.19 71.89
1.19 No. 16 40.52 1449.28 96.35 3.65 27.13 1395.90 93.79 6.21 4.93 51.27
0.59 No. 30 23.67 1472.95 97.92 2.08 40.41 1436.31 96.51 3.49 2.78 40.91
0.279 No. 50 16.76 1489.71 99.04 0.96 32.11 1468.42 98.67 1.33 1.15 31.83
0.149 No. 100 14.46 1504.17 100.00 0.00 19.83 1488.25 100.00 0.00 0.00 22.14
0.074 No. 200 0.00 1504.17 100.00 0.00 0.00 1488.25 100.00 0.00 0.00 11.03
Pan
BERAT CONTOH 1504.17 Gram 1488.25 Gram

Pekerjaan / Proyek : Pelebaran Ruas Kapuk - Pluit / Tol CTCSample : Lab. Crew Tanggal : 25/04/2015
Jenis Material : Hot Bin III / Trial Mix Batch Dikerjakan : Handita Tanggal : 25/04/2015
Sumber Material : AMP Cakung - Jakarta Diperiksa : T. Hidayat Tanggal : 25/04/2015

TEST 1 TEST 2
ASTM Berat Berat Average
KUMULATIF KUMULATIF
SIEVE tertahan tertahan Prosentase
SIZE Masing 2 Berat Prosentase Prosentase Masing 2 Berat Prosentase Prosentase Lolos Keterangan
Saringan Tertahan Tertahan Lolos Saringan Tertahan Tertahan Lolos
mm inch gram gram % % gram gram % % %
50.0 2" 0.00 0.00 0.00 100.00 0.00 0.00 0.00 100.00 100.00
37.5 1 1/2" 0.00 0.00 0.00 100.00 0.00 0.00 0.00 100.00 100.00
25.4 1" 0.00 0.00 0.00 100.00 0.00 0.00 0.00 100.00 100.00 100.00
19.1 3/4" 0.00 0.00 0.00 100.00 0.00 0.00 0.00 100.00 100.00 100.00
12.7 1/2" 248.17 248.17 13.78 86.22 292.37 292.37 16.40 83.60 84.91 100.00
9.5 3/8" 1147.63 1395.80 77.53 22.47 1135.67 1428.04 80.11 19.89 21.18 100.00
4.76 No. 4 293.14 1688.94 93.81 6.19 282.88 1710.92 95.98 4.02 5.10 99.47
2.38 No. 8 46.12 1735.06 96.37 3.63 33.23 1744.15 97.85 2.15 2.89 71.89
1.19 No. 16 23.85 1758.91 97.70 2.30 17.12 1761.27 98.81 1.19 1.75 51.27
0.59 No. 30 20.69 1779.60 98.85 1.15 10.22 1771.49 99.38 0.62 0.89 40.91
0.279 No. 50 20.78 1800.38 100.00 0.00 11.01 1782.50 100.00 0.00 0.00 31.83
0.149 No. 100 0.00 1800.38 100.00 0.00 0.00 1782.50 100.00 0.00 0.00 22.14
0.074 No. 200 0.00 1800.38 100.00 0.00 0.00 1782.50 100.00 0.00 0.00 11.03
Pan
BERAT CONTOH 1800.38 Gram 1782.50 Gram
STABILITY CORRELATION RATIOS

Volume of Approximate Thickness Correlation


Specimen, of Specimen, Ratio

cm3 inch mm

200 to 213 1 25.4 5.56


214 to 225 1 1/16 27.0 5.00
226 to 237 1 1/8 28.6 4.55
238 to 250 1 3/16 30.2 4.17
251 to 264 1 1/4 31.8 3.85
265 to 276 1 5/16 33.3 3.57
277 to 289 1 3/8 34.9 3.33
290 to 301 1 7/16 36.5 3.03
302 to 316 1 1/2 38.1 2.78
317 to 328 1 9/16 39.7 2.50
329 to 340 1 5/8 41.3 2.27
341 to 353 1 11/16 42.9 2.08
354 to 367 1 3/4 44.4 1.92
368 to 379 1 13/16 46.0 1.79
380 to 392 1 7/8 47.6 1.67
393 to 405 1 15/16 49.2 1.56
406 to 420 2 50.8 1.47
421 to 431 1 1/16 52.4 1.39
432 to 443 2 1/8 54.0 1.32
444 to 456 2 3/16 55.6 1.25
457 to 470 2 1/4 57.2 1.19
471 to 482 2 5/16 58.7 1.14
483 to 495 2 3/8 60.3 1.09
496 to 508 2 7/16 61.9 1.04
509 to 522 2 1/2 63.5 1.00
523 to 535 2 9/16 64.0 0.96
536 to 546 2 5/8 65.1 0.93
547 to 559 2 11/16 66.7 0.89
560 to 573 2 3/4 68.3 0.86
574 to 585 2 13/16 71.4 0.83
586 to 598 2 7/8 73.0 0.81
599 to 610 2 15/16 74.6 0.78
611 to 625 3 76.2 0.76