You are on page 1of 1

JAYASHREE POLYMERS PVT.LTD.

PROCESS CAPABILITY STUDY

PART NO. ::: SEALING FRAME PARAMETER :: Diameter Date :: 14-Dec-20 Initial (Ppk, Pp)
Ongoin
PART NAME ::: PV465001 / CE4KB01 A 01 SPCEFICATION :: Ø3.00 ± 0.15 mm (Cpk, Cp)
M/s- MAHLE ANAND Thermal
SUPPLIER ::: Systems Private Limited USL = 3.15 mm Sub Group Size = 5 Doc No : - F10QA52
LSL = 2.85 mm Rev 03 Date : - 02-08-2019
INSTRUMENT NAME : Thickness Gauge
INSTRUMENT SIZE : 0~10mm
Sl.No. 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25

Reading 1 2.99 3.03 3.00 2.99 3.03 3.01 3.02 3.06 3.05 3.02
Reading 2 3.01 3.05 3.01 3.00 3.07 3.00 2.99 3.01 3.02 2.99
Reading 3 3.03 3.01 3.03 3.01 3.02 3.05 3.04 3.00 3.00 3.04
Reading 4 3.06 3.00 3.05 3.02 3.04 3.02 3.04 3.00 2.98 3.04
Reading 5 3.04 2.99 3.07 3.08 3.02 2.98 3.05 2.99 3.05 3.01

Average 3.03 3.02 3.03 3.02 3.04 3.01 3.03 3.01 3.02 3.02 n.a n.a n.a n.a n.a n.a n.a n.a n.a n.a n.a n.a n.a n.a n.a
Range 0.07 0.06 0.07 0.09 0.05 0.07 0.06 0.07 0.06 0.05 n.a n.a n.a n.a n.a n.a n.a n.a n.a n.a n.a n.a n.a n.a n.a
Date of Samples taken for
Measurement

Average Chart LCL UCL n = 5


3.50
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 X (Doubl. Bar) = 3.02 X --- 2.99 3.06 A2 = 0.58 D4 = 2.11
3.00
R (Bar) = 0.06 Range- 0 0.13 D3 = 0 d2 = 2.33
2.50 Average R (Bar) /d2 = 0.027
2.00
USL
STDEV = 0.025 Remarks :
LSL

UCL(x)
Sigma = 0.025 {1} PROCESS IS STABLE
1.50
LCL(x) Initial Study PROCESS CAPABILITY
1.00 X(D.B)
Pp 2.004 {2} EXCELLENT
0.50 Z(usl)/3 = 1.699
Z(lsl)/3 = 2.3 {3} ___
0.00
Ppk 1.699
Range Chart
0.16
0.14
0.12
Range
0.10
UCL(R)
0.08
LCL(R)
0.06
R (Bar)
0.04
0.02 Vijay B Shankar
0.00 PREPARED BY : APPROVED BY :
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25