You are on page 1of 4

SAUDI ARAMCO ID/PIEU - 30-Apr-2017 - REV. 2015.03.00 (Standards Cutoff - March 2015) Rev. 2015.03.

00 31-Mar-15
SAIC NUMBER DATE APPROVED QR NUMBER
SAUDI ARAMCO INSPECTION CHECKLIST
In-Process Inspection of FBE coating Application on External
Field Girth Welds [Includes Repair / Patch-up coating]
SAIC-H-2015 30-Apr-17 Coating-
PROJECT TITLE WBS / BI / JO NUMBER CONTRACTOR / SUBCONTRACTOR

EQUIPMENT ID NUMBER(S) EQUIPMENT DESCRIPTION EQPT CODE SYSTEM ID. PLANT NO.

LAYOUT DRAWING NUMBER REV. NO. PURCHASE ORDER NUMBER EC / PMCC / MCC NO.

SCHEDULED INSPECTION DATE & TIME ACTUAL INSPECTION DATE & TIME QUANTITY INSP. MH's SPENT TRAVEL TIME
SAUDI ARAMCO USE ONLY
SAUDI ARAMCO TIP NUMBER SAUDI ARAMCO ACTIVITY NUMBER WORK PERMIT REQUIRED?

SAUDI ARAMCO INSPECTION LEVEL CONTRACTOR INSPECTION LEVEL

ITEM
ACCEPTANCE CRITERIA REFERENCE PASS FAIL N/A RE-INSP DATE
No.

A General Requirements (Limited to APCS 104 System Application)

Coating applicator is certified & working to an approved procedure, SAEP-316,


A1
using the APCS 104 Para. 3.1

SAES-H-201,
FBE coating powder complies with the requirements of APCS-104,
A2 Para. 5.3
verified by receiving records and material markings
Para. 6.1

The repair material i.e. FBE powder, melt sticks, liquid coatings, are SAES-H-201,
A3
approved by FBE coating supplier and approved by CSD. Para. 8.5.3

SAES-H-201,
A4 Coating equipment is working properly as verified by SAIC-H-2013 Para. 7.3.5.1

FBE Powder application is not performed during periods of bad SAES-H-201,


A5 weather (rain, high winds, etc.) Para. 7.3.6
except when satisfactory protective canopies are provided.

B Heating of Pipe Surface:

Blasted area showing evidence of flash rusting are re-blasted prior to SAES-H-201,
B1
heating. Para. 7.3.2

Pipe surface was heated to a temperature specified by the Powder SAES-H-201,


B2
Manufacturer using an induction heating coil. (Req'd Temp=______ ) Para. 7.3.3

Metal temperature was measured with contact pyrometers or


equivalent (Or with digital/laser type thermometer).
SAES-H-201,
B3 Note: Para. 7.3.4
A)Temperature crayons are not allowed and are not used Para. 7.3.3
B) Verify that adjacent coating are not damaged due to
excessive temperatures.

C FBE Powder Application:

Powder application is performed as soon as the induction heater coil SAES-H-201,


C1
is removed. Para. 7.3.5

The machine shall apply powder to a uniform rate, to a correct width


centered on the girth weld, to a dry film thickness of 625 to 1000 SAES-H-201,
C2
microns in the least number of passes as demonstrated in the Para. 7.3.5.1
Checklist # SAIC-H-2013.

Dirt or other deleterious foreign material shall not contaminate the SAES-H-201,
C3
powder coated area during application and curing stages. Para. 7.3.5.2

Freshly patched coated areas shall be allowed to cure according to SAES-H-201,


C4
Manufacturer's recommendations prior to handling Para. 8.5.3

Saudi Aramco: Company General Use


SAUDI ARAMCO ID/PIEU - 30-Apr-2017 - REV. 2015.03.00 (Standards Cutoff - March 2015) Rev. 2015.03.00 31-Mar-15
SAIC NUMBER DATE APPROVED QR NUMBER
SAUDI ARAMCO INSPECTION CHECKLIST
In-Process Inspection of FBE coating Application on
External Field Girth Welds [Includes Repair / Patch-up SAIC-H-2015 30-Apr-17 Coating-
coating]
PROJECT TITLE WBS / BI / JO NUMBER CONTRACTOR / SUBCONTRACTOR

EQUIPMENT ID NUMBER(S) EQUIPMENT DESCRIPTION EQPT CODE SYSTEM ID. PLANT NO.

LAYOUT DRAWING NUMBER REV. NO. PURCHASE ORDER NUMBER EC / PMCC / MCC NO.

SCHEDULED INSPECTION DATE & TIME ACTUAL INSPECTION DATE & TIME QUANTITY INSP. MH's SPENT TRAVEL TIME
SAUDI ARAMCO USE ONLY
SAUDI ARAMCO TIP NUMBER SAUDI ARAMCO ACTIVITY NUMBER WORK PERMIT REQUIRED?

SAUDI ARAMCO INSPECTION LEVEL CONTRACTOR INSPECTION LEVEL

ITEM
ACCEPTANCE CRITERIA REFERENCE PASS FAIL N/A RE-INSP DATE
No.

D Visual Inspection:

The quality of cure shall be checked on the first 5 joints of the job
and twice each day thereafter by maintaining a MEK soaked pad
in contact with the coating surface for one minute and then SAES-H-201,
D1
rubbing vigorously for 15 seconds. Para. 8.2.3
There shall be no softening of the coating or substantial color
removal from the coating.

SAES-H-201,
D2 The finished coating shall have a uniform, glossy appearance.
Para. 8.2.4

Coating surface is free of coating defects such as visible SAES-H-201,


D3
holidays, fish eyes, lumps, dry spray, runs & sags. Para. 8.2.4
Width of covered area is as per Powder Manufacturers
Instruction/Procedure but not less than 280 mm centered on the SAES-H-201,
D4 weld. (Indicate Manufacturer's required width = __________ ) Para. 6.2

Coating overlap shall be within the thickness specified in SAES-


H-200 and / or as per the applicator's procedure approved. SAES-H-201,
D5
Para. 8.2.4

E Dry Film Thickness (DFT) measurement:

A minimum of six (6) DFT readings are taken on each field joint
coating including readings on the weld seam. SAES-H-201,
E1
Note: Thickness gauge shall be calibrated in accordance with Para. 8.2.2
SSPC PA-2

SAES-H-201,
E2 Dry Film Thickness (DFT) shall be 625 to 1000 microns.
Para. 7.3.5.1

F Holiday Testing and Adhesion Test


The coated girth weld surface area is 100% Holiday tested as
per SAIC-H-2016. SAES-H-201,
All holidays, imperfections, and damaged areas are carefully Para.8.3.1
identified and marked with a waterproof marker. &
F1
para. 8.3.2
SAES-H-200
Para. 7.1

Saudi Aramco: Company General Use


SAUDI ARAMCO ID/PIEU - 30-Apr-2017 - REV. 2015.03.00 (Standards Cutoff - March 2015) Rev. 2015.03.00 31-Mar-15
SAIC NUMBER DATE APPROVED QR NUMBER
SAUDI ARAMCO INSPECTION CHECKLIST
In-Process Inspection of FBE coating Application on
External Field Girth Welds [Includes Repair / Patch-up SAIC-H-2015 30-Apr-17 Coating-
coating]
PROJECT TITLE WBS / BI / JO NUMBER CONTRACTOR / SUBCONTRACTOR

Coating adhesion test is conducted as follows:


A) An X incision is made on coating up to metal substrate using a
sharp knife.
SAES-H-201,
B) Coating is pealed at the intersection of X using the knife point.
Para. 8.4.1
F2 C) Refusal of the coating to peel constitutes a PASS.
&
D) Partial or complete adhesion failure between the
Para. 8.4.2
coating and the metal substrate constitutes a failure. Cohesive
failure caused by voids in the coating leaving a honeycomb
structure on the specimen surface also constitutes failure.

If the coating fails adhesion test adjacent field girth weld areas
shall also be tested until acceptable coatings are found on both
sides of the defective coating. SAES-H-201,
F3
The defective coatings shall all be completely removed and the Para. 8.4.4
areas recoated. At least one of the repaired areas shall be re-
inspected.

The Adhesion test is performed once every hour.


SAES-H-201,
F4 Note: When five consecutive tests are successful, the frequency
Para. 8.4.3
shall be reduced to once every two hours.

G Repairs

All holidays, imperfections, and damaged areas are carefully SAES-H-201,


G1
identified and marked with a waterproof marker. Para. 8.3.2

Girth welds showing more than 3 holidays shall be completely SAES-H-201,


G2
blasted off and the area recoated. Para. 8.5.1

Pipe surface to be repaired are cleaned to remove all dirt and


damaged or disbonded coating using abrasive blasting or other
approved and suitable means. SAES-H-201,
G3
The edges of the original coatings shall be "feathered out" Para. 8.5.2
approximately 50 mm around the specific area to be
coated, and all dust wiped off before applying the patch coating.

Freshly patched coated areas shall be allowed to cure according SAES-H-201,


G4
to Manufacturer's recommendations prior to handling Para. 8.5.3

Patch repair areas shall be 100% holiday tested in accordance


SAES-H-201,
G5 as E1 above. No holidays shall be present on the girth weld after
Para. 8.5.4
patching.
Remarks:
REFERENCE DOCUMENTS:
1. SAES-H-201: General Spec for Over-the-Ditch Ext and Int FBE Coating of Field Girth Welds (16 November 2011)

2. SAES-H-001: Coating Selection & Application Requirements for Industrial Plants & Equipment, (10 April 2011).
3. SAEP 316: Performance Qualification of coating personnel (11 Mar. 2015)
4. SAES-H-200: Storage, Handling and Installationof Externally Coated Pipe (24 October 2011)
Contractor / Third-Party Saudi Aramco
Construction Representative* PMT Representative
Work is Complete and Ready for Inspection: T&I Witnessed QC Record Reviewed Work Verified
Name, Initials and
Name, Initials and Date:
Date:

QC Inspector PID Representative


Performed Inspection Work / Rework May Proceed T&I Witnessed QC Record Reviewed Work Verified
Name, Initials and
Name, Initials and Date:
Date:

QC Supervisor Proponent and Others

Saudi Aramco: Company General Use


SAUDI ARAMCO ID/PIEU - 30-Apr-2017 - REV. 2015.03.00 (Standards Cutoff - March 2015) Rev. 2015.03.00 31-Mar-15
SAIC NUMBER DATE APPROVED QR NUMBER
SAUDI ARAMCO INSPECTION CHECKLIST
In-Process Inspection of FBE coating Application on
External Field Girth Welds [Includes Repair / Patch-up SAIC-H-2015 30-Apr-17 Coating-
coating]
PROJECT TITLE WBS / BI / JO NUMBER CONTRACTOR / SUBCONTRACTOR

Quality Record Approved: T&I Witnessed QC Record Reviewed Work Verified


Name, Organization,
Name, Sign and Date:
Initials and Date:

*Person Responsible for Completion of Quality Work / Test Y = YES N = NO F = FAILED

Saudi Aramco: Company General Use

You might also like