INDIA CRETE RMC

Plant : DEONER PLANT Date 05-10-2021


Client Ajmera Realty & Infra India Ltd Project : Ajmera Island
A. Mix Stipulation
Grade of Concrete M 40 Pile Workability (FLOW) 200 + 25 mm
Maximum Size of Aggregate 20 mm Exposure type SEVERE
Cement Type OPC 53 Method of Concrete Placing Pumping
Mineral Admixture Used FLYASH
Type of Concrete RCC

Characteristic Compressive Strength @ 28 days : 40 N/mm2

B. Target Strength
( Assumed Std Dev 5.0 as per IS 456:2000 Table 8)
Target Mean Strength = (fck+ t x SD)
= 40+1.65x5
= 48.25 N/mm2

C . Ingredient Data

Specific
Ingredient Type Source - Supplier Absorption
Gravity

Cement OPC 53 ULTRATECH/ACC/AMBUJA 3.15 -


FLYASH DAHANU ASHTECH 2.22 -
Mineral Addition
MICROSILICA 2.6 -
20 mm URAN 2.8 1.15%
Coarse Aggregate
10 mm URAN 2.79 1.45%
-
Fine Aggregate
Cr. Sand URAN 2.69 4.80%
CAC HYPERFLUID CAC 1.088 -
Admixture CAC RETARDPLAST CAC 1.11 -
-

Notes

( QC Incharge)
D . Ingredient Quantity (kg) for 1 m3 Concrete ( SSD Mix Design)
Design Mix Proportion
OPC 53 420
FLYASH 110 1
0 % by Weight
20 mm 402 0.76 23%
51%
10 mm 490 0.92 28%
0 0.00 0%
Cr. Sand 857 1.62 49% 49%
Effective Water 155 0.29
Admixtures
CAC HYPERFLUID 4.24 0.80% ±0.5%
CAC RETARDPLAST 3.18 0.60% +0.25%
0 0.00%
Total wt 2441

F . Mix after Absorption ( Dry Mix design )


Description SSD Qty (Kg/m3) Absorption Dry Qty (Kg/m3)
OPC 53 = 420 = 420
FLYASH = 110 = 110
20 mm = 402 - 5 = 398
10 mm = 490 - 7 = 483
Cr. Sand = 857 - 41 = 816
Total Water = 155 + 53 = 208
CAC HYPERFLUID
= 4.24 = 4.2
CAC RETARDPLAST
= 3.18 = 3.2
Total wt = 2441 = 2441

Notes
This mix design is based on the available material. In future, if there is any change in the material ( ±5%), we shall make changes