You are on page 1of 2

WPSasme-FNC-UTI-001A-2019_CS_0.

5_GTAW FOR WELDER QUALIFICATION

01
00
00
01
WELDING PROCEDURE WPS Nr. 40UT-19.370.3 REV.
QUALIFICATION Date 8/08/2019
WPS Supporting PQR 01A/11
According ASME BPVC Sec. IX

Welding Process(es) 1 GTAW 2 - 3 -

Type(s) 1 MANUAL 2 - 3 -
(Manual, Automatic, Semi-Automatic)

JOINTS (QW-402)
DETAILS
75°

Tk 0,393 Max.
1

3/32" Max 2

5/32" Max.
Joint Design Single V Groove (See details)
Backing (Yes/No) No
Backing Material (Type) None

Metal
Nonfusing Metal
Non Metallic
Other

(1)
BASE METALS (QW-403)

P - Nr. : 1 Group : 1&2 To P - Nr. : 1 Group : 1&2


OR
Specification Type : N/A Grade : N/A To Specification Type : N/A Grade : N/A
OR
Chem. Analysis : N/A And Mech. Property : N/A
To Chem. Analysis : N/A And Mech. Property : N/A
BASE METAL: THICKNESS / DIAMETER RANGE :
Thickness Range : Groove : 0,0625" - 0,393" And Fillet : All
Pipe Diam. Range : Groove : All And Fillet : All
Maximum Pass Thickness ≤1/2" (Yes/No): Yes
Other : None

FILLER METALS (QW-404) ( 1 )

1 2 3
SFA Specification Nr. : SFA 5.18 - -
AWS Class Nr. : ER 70S-6 - -
F-Nr. : 6 - -
A-Nr. : 1 - -
Size of Filler Metals : 3/32", 1/8" - -
Filler metal product form Bare (Solid) - -
Deposited W. Metal Thk. Range Groove : 0,393 Max. - -
Deposited W. Metal Thk. Range Fillet : All - -
Electrode / Flux : N/A - -
Flux Trade Name : N/A - -
Consumable Insert : N/A - -
Other : Trade Name N/A - -
Manufacturer N/A -- --

(1)
= Each base metal / filler metal combination should be recorded individually. Page 1 of 2

WPSasme-FNC-UTI-001A-2019_CS_0.5_GTAW Pagina 1
FOR WELDER QUALIFICATION

WELDING PROCEDURE WPS Nr. 40UT-19.370.3 REV.


01
00
00
01
QUALIFICATION Date 8/08/2019
WPS Supporting PQR 01A/11
According ASME BPVC Sec. IX
POSITION (QW-405) POSTWELD HEAT TREATMENT (QW-407)

Position of Groove : All Temperature : N/A


Weld Progrssion (Uphill, Downhill) : Uphill Time : N/A
Position of Fillet : All Other : N/A

PREHEAT (QW-406) GAS (QW-408) % Composition


Gas(es) (Mixture) Flow Rate
Preheat Temperature Min. : 50°F Shielding Argon 99,99 20-50 CFH
Interpass Temperature Max. : 600°F Max. Trailing N/A N/A N/A
Preheat Maintenance : Held til completion of joint Backing N/A N/A N/A
Other :
ELECTRICAL CHARACTERISTICS (QW-409)

Weld Layer(s) Process Filler Metal Current Volts Range (V) Travel Speed Heat Imput
Class Diameter (in) Type / Polarity Amps Range (A) Range (mm/min.) Ran.(J/mm)
1-n GTAW ER 70S-6 3/32", 1/8" DCEN 70-180 20-30 Manual N/A

Tungsten Electode Size and Type : 1/8",thoriated 2%,A5.12 EWHT-2


Mode of Metal Transfer for GMAW : N/A

TECNIQUE (QW-410)

String or Weave Bead : Both


Orifice or Gas Cup Size : #6 - #12
Initial and Interpass Cleaning : Brushing and grinding.
Method of Back Gouging : None
Oscillation : N/A
Contact Tube to Work Distance : N/A
Multiple or Single P. (x side) : Multiple
Multiple or Single Electrodes : Single
Travel Speed (Range) : Manual
Peening : N/A
Other : None

Notes:

Issued by: Arnold Batista Date: 10/08/2019 Sign:

Last revision by: Abraham Perea Date: 13/08/2019 Sign:

Page 2 of 2

WPSasme-FNC-UTI-001A-2019_CS_0.5_GTAW Pagina 2