TYPE OF SAMPLE 10 mm
DATE OF SAMPLE 9/24/2018
SIEVE ANALYSIS FOR 20 MM WBM METAL
WT. OF SAMPLE TAKEN 13679 gm (IS:383 Tab.2)
I.S.Sieve Commulative
Wt.Retained %age Specified limit
Sr.No. Designation %age %age of passing
in gm. Retained (%age)
No. Retained
1 40 mm 0 0 0 100 100%
2 20 mm 0 0.00 0.00 100.00 100%
3 10 mm 9465 69.19 69.19 30.81 0-45%
4 4.75 mm 4125 30.16 99.35 0.65 0-10%
5 Pan 89 0.65 100.00 0
Total 13679 100.00
SIZE OFAGGREGATE
Thickness of
Passsing Wt. of fraction consisting at Wt. of aggregate in each fraction
Sr.No. Retained on guage size in
through IS least 200 pieces passing through guage
IS Sieve mm
Sieve
1 63 mm 50 mm W1 33.9 W1
2 50 mm 40 mm W2 27 W2
3 40 mm 25 mm W3 19.5 W3
4 25 mm 20 mm W4 13.5 W4
5 20 mm 16 mm W5 10.8 W5
6 16 mm 12.5 mm W6 8.55 W6
7 12.5 mm 10 mm W7 6.75 W7
8 10 mm 6.3mm W8 4.89 W8
TOTAL W W*
FLAKINESS INDEX (W*/W)X100 = /
REFERANCE :-IS 2386 PART I, MOST 2000, IS 383, PWD STD. SPECIFICATION
Assist.Reaserch Officer,
Vigilance & Quality Control(P.W.),
Dist.Laboratory,Ahmednagar
VIGILANCE & QUALITY CONTROL CIRCLE NASHIK
DIST. LABORATORY, AHMEDNAGAR
TEST DATA SHEET:DCASP&Wa-08
Assist.Reaserch Officer,
Vigilance & Quality Control(P.W.),
Dist.Laboratory,Ahmednagar
VIGILANCE & QUALITY CONTROL CIRCLE NASHIK
DIST. LABORATORY, AHMEDNAGAR
TEST DATA SHEET:DCAI-11
JOB NO. AHA/18-19/ 488 / PW/SNR
NAME OF DIVISION Public Work Divi. Sangamner
NAME OF SUBDIVISION P.W.SubDivision Akole-1
NAME OF WORK Concreting Sangavi To Dagadwadi Road Tal- Akole.
Assist.Reaserch Officer,
Vigilance & Quality Control(P.W.),
Dist.Laboratory,Ahmednagar
DIST. LABORATORY, AHMEDNAGAR
JOB NO. AHA/18-19/ 488 / PW/SNR LAB./NO./SNR:- DATE:-
NAME OF DIVISION P.W.SubDivision Sangamner
NAME OF SUBDIVISION P.W.Sub Division Akole-1
NAME OF WORK Concreting Sangavi To Dagadwadi Road Tal- Akole.
40 MM 100 100%
20 MM 100.00 100%
Pan 0.00 0
Result Obtained
Sr. No. Type of Test Result Specified for WBM Remark
20 MM METAL Trap Laterite
BRICKS TEST
JOB NO. AHA/22-23 / 926 / PW/ANR
NAME OF DIVISION Public Work Division Ahmednagar
NAME OF SUBDIVISION Public Work Sub. Division Parner
NAME OF WORK S.R. to Bridge on SH-54 to Rashin Alsunde Nimbe Khatgaon Loni Masadppur to MDR 8
Chapadgaon road, MDR.101 @ Km 1/100 tal- Karjat Dist- Ahmednagar
TYPE OF SAMPLE :-Bricks
DATE OF RECPT. OF SAMPLE 9/29/2018
DATE OF TESTING 29/09/2018 to 04/10/2018
Efflorescence
As there is 10 % perciptable residue or deposit on surface of brick after keeping both the ends of brick in water for 24 hours .
Hence effloerance is Slight
4 ……do…… 230x100X75 21.28% 3.22 For IInd Class For Iind Class
For IInd Class
5 ……do…… 230x100X75 21.10% 3.04 Not Less Not Less
Not More
Than 3.93 Than 2.95
Than 22 %
Average 21.21% Average 3.13 N/mm² N/mm²
As there is 10 % perciptable residue or deposit on surface of brick after keeping both the ends of brick in water for 24 hours . Hence effloerance is Slight
Note :-The test result based on samples received in the Laboratory
Reference : :- I.S.3495 ( Part (I), (II) 1992
I.S.Sieve Commulative
Wt.Retained %age Specified limit
Sr.No. Designation %age %age of passing
in gm. Retained (%age)
No. Retained
1 40 mm 0 0 0 100 100%
2 20 mm 263 2.93 2.93 97.07 85-100 %
3 10 mm 7081 78.83 81.75 18.25 0-20 %
4 4.75 mm 1458 16.23 97.99 2.01 0-5 %
5 Pan 181 2.01 100.00 0
Total 8983 100.00
SIZE OFAGGREGATE
Thickness of
Passsing Wt. of fraction consisting at Wt. of aggregate in each fraction
Sr.No. Retained on guage size in
through IS least 200 pieces passing through guage
IS Sieve mm
Sieve
1 63 mm 50 mm W1 33.9 W1
2 50 mm 40 mm W2 27 W2
3 40 mm 25 mm W3 19.5 W3
4 25 mm 20 mm W4 13.5 W4
5 20 mm 16 mm W5 10.8 W5
6 16 mm 12.5 mm W6 8.55 W6
7 12.5 mm 10 mm W7 6.75 W7
8 10 mm 6.3mm W8 4.89 W8
TOTAL W W*
FLAKINESS INDEX (W*/W)X100 = /
REFERANCE :-IS 2386 PART I, MOST 2000, IS 383, PWD STD. SPECIFICATION
Assist.Reaserch Officer,
Vigilance & Quality Control(P.W.),
Dist.Laboratory,Ahmednagar
VIGILANCE & QUALITY CONTROL CIRCLE NASHIK
DIST. LABORATORY, AHMEDNAGAR
TEST DATA SHEET:DCASP&Wa-08
Assist.Reaserch Officer,
Vigilance & Quality Control(P.W.),
Dist.Laboratory,Ahmednagar
VIGILANCE & QUALITY CONTROL CIRCLE NASHIK
DIST. LABORATORY, AHMEDNAGAR
TEST DATA SHEET:DCAI-11
JOB NO. AHA/22-23 / 926 / PW/ANR
NAME OF DIVISION Public Work Divi. Ahmednagar
NAME OF SUBDIVISION P.W.Sub Division Parner
NAME OF WORK S.R. to Bridge on SH-54 to Rashin Alsunde Nimbe Khatgaon Loni
Masadppur to MDR 8 Chapadgaon road, MDR.101 @ Km 1/100 tal-
Karjat Dist- Ahmednagar
TYPE OF SAMPLE :- 20 MM METAL
DATE OF SAMPLE 9/29/2018
DATE OF TESTING 43372
Assist.Reaserch Officer,
Vigilance & Quality Control(P.W.),
Dist.Laboratory,Ahmednagar
DIST. LABORATORY, AHMEDNAGAR
JOB NO. AHA/22-23 / 926 / PW/ANR LAB./NO./ANR:- DATE:-
NAME OF DIVISION P.W.Sub Division Ahmednagar
NAME OF SUBDIVISION P.W.Sub Division Parner
NAME OF WORK S.R. to Bridge on SH-54 to Rashin Alsunde Nimbe Khatgaon Loni Masadppur to MDR 8 Chapadgaon road, MDR.101 @ Km 1/100 tal- Karjat Dist-
Ahmednagar
TYPE OF SAMPLE :- 20 MM METAL
DATE OF SAMPLE 9/29/2018
DATE OF TESTING 9/29/2018
40 MM 100 100%
20 MM 97.07 85-100%
4.75 MM 2.01 0- 5%
Pan 0.00 0
1 2 3 4 5 6 7 8 9 10 11 12 13 14
2 S-2 M-20 12/2/2018 12/27/2018 25 150x150x150 22500 8.462 480 21.33 20.89 19.60
5 C-2 M-20 12/2/2018 12/27/2018 25 150x150x150 22500 8.459 470 20.89 21.19 19.60
2 A-2 M-20 9/14/2018 11/1/2018 48 150x150x150 22500 8.499 500 22.22 21.93 21.00
1 2 3 4 5 6 7 8 9 10 11 12 13 14
2 D-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 8475 870 38.67 32.15 30.00 e
5 E-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 8546 690 30.67 31.85 30.30 f
2 F-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 8475 690 30.67 30.52 30.15 g
5 G-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 8546 700 31.11 31.41 30.00 h
1 2 3 4 5 6 7 8 9 10 11 12 13 14
2 H-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 8475 790 35.11 32.15 30.00 i
5 I-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 8546 750 33.33 31.85 30.00 j
2 J-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 8475 690 30.67 32.59 30.00 k
5 K-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 8546 710 31.56 32.30 30.00 l
1 2 3 4 5 6 7 8 9 10 11 12 13 14
2 M-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 8475 225 10.00 10.00 10.00 m
5 N-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 8546 225 10.00 10.00 20.00 n
2 P-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 8475 352 15.64 15.97 15.00 o
5 R-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 8546 352 15.64 15.64 16.00 p
1 2 3 4 5 6 7 8 9 10 11 12 13 14
2 A-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 8475 352 15.64 15.97 17.00 q
5 B-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 8546 352 15.64 15.64 18.00 r
2 M-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 8475 352 15.64 15.97 19.00 s
5 N-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 8546 352 15.64 15.64 20.00 t
1 2 3 4 5 6 7 8 9 10 11 12 13 14
2 P-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 8475 352 15.64 15.97 21.00 u
5 R-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 8546 352 15.64 15.64 22.00 v
2 J-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 8475 352 15.64 15.97 23.00 w
5 K-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 8546 352 15.64 15.64 24.00 x
1 2 3 4 5 6 7 8 9 10 11 12 13 14
2 A-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 8475 352 15.64 15.97 25.00 y
5 B-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 8546 352 15.64 15.64 26.00 z
2 D-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 8475 352 15.64 15.97 27.00 a
5 E-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 8546 352 15.64 15.64 28.00 b
Average Reqd.
Grade of Age of Compressiv Compressive
Sr. Identification Dimension of Cross sectional Compre. Comp.
Concrete Date of casting Date of Testing Specimen in e Load in Strenght Remarks
No. Mark Specimen in mm Area in sqmm Strenght Strenght h
mix Days kN inN/sqmm
inN/sqmm in N/sqmm
1 2 3 4 5 6 7 8 10 11 12 13 14
2 S-2 M-20 12/2/2018 12/27/2018 25 150x150x150 22500 480 21.33 20.89 19.60
5 C-2 M-20 12/2/2018 12/27/2018 25 150x150x150 22500 470 20.89 21.19 19.60
Average Reqd.
Age of Compressiv Compressive
Identification Concrete Dimension of Cross sectional Compre. Comp.
Sr.No. Date of casting Date of Testing Specimen in e Load in Strength Remarks
Mark mix Specimen in mm Area in sqmm Strenght Strength in
Days kN inN/sqmm
inN/sqmm N/sqmm
1 2 3 4 5 6 7 8 10 11 12 13 14
2 A-2 M-20 9/14/2018 11/1/2018 48 150x150x150 22500 500 22.22 21.93 21.00
Average Reqd.
Grade of Age of Compressiv Compressive
Sr. Identification Dimension of Cross sectional Compre. Comp.
Concrete Date of casting Date of Testing Specimen in e Load in Strenght Remarks
No. Mark Specimen in mm Area in sqmm Strenght Strenght h
mix Days kN inN/sqmm
inN/sqmm in N/sqmm
1 2 3 4 5 6 7 8 10 11 12 13 14
2 D-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 870 38.67 32.15 30.00 e
5 E-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 690 30.67 31.85 30.30 f
Average Reqd.
Age of Compressiv Compressive
Identification Concrete Dimension of Cross sectional Compre. Comp.
Sr.No. Date of casting Date of Testing Specimen in e Load in Strength Remarks
Mark mix Specimen in mm Area in sqmm Strenght Strength in
Days kN inN/sqmm
inN/sqmm N/sqmm
1 2 3 4 5 6 7 8 10 11 12 13 14
2 F-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 690 30.67 30.52 30.15 g
5 G-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 700 31.11 31.41 30.00 h
Average Reqd.
Grade of Age of Compressiv Compressive
Sr. Identification Dimension of Cross sectional Compre. Comp.
Concrete Date of casting Date of Testing Specimen in e Load in Strenght Remarks
No. Mark Specimen in mm Area in sqmm Strenght Strenght h
mix Days kN inN/sqmm
inN/sqmm in N/sqmm
1 2 3 4 5 6 7 8 10 11 12 13 14
2 H-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 790 35.11 32.15 30.00 i
5 I-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 750 33.33 31.85 30.00 j
Average Reqd.
Age of Compressiv Compressive
Identification Concrete Dimension of Cross sectional Compre. Comp.
Sr.No. Date of casting Date of Testing Specimen in e Load in Strength Remarks
Mark mix Specimen in mm Area in sqmm Strenght Strength in
Days kN inN/sqmm
inN/sqmm N/sqmm
1 2 3 4 5 6 7 8 10 11 12 13 14
2 J-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 690 30.67 32.59 30.00 k
5 K-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 710 31.56 32.30 30.00 l
Average Reqd.
Grade of Age of Compressiv Compressive
Sr. Identification Dimension of Cross sectional Compre. Comp.
Concrete Date of casting Date of Testing Specimen in e Load in Strenght Remarks
No. Mark Specimen in mm Area in sqmm Strenght Strenght h
mix Days kN inN/sqmm
inN/sqmm in N/sqmm
1 2 3 4 5 6 7 8 10 11 12 13 14
2 M-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 225 10.00 10.00 10.00 m
5 N-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 225 10.00 10.00 20.00 n
Average Reqd.
Age of Compressiv Compressive
Identification Concrete Dimension of Cross sectional Compre. Comp.
Sr.No. Date of casting Date of Testing Specimen in e Load in Strength Remarks
Mark mix Specimen in mm Area in sqmm Strenght Strength in
Days kN inN/sqmm
inN/sqmm N/sqmm
1 2 3 4 5 6 7 8 10 11 12 13 14
2 P-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 352 15.64 15.97 15.00 o
5 R-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 352 15.64 15.64 16.00 p
16.00 p
Average Reqd.
Grade of Age of Compressiv Compressive
Sr. Identification Dimension of Cross sectional Compre. Comp.
Concrete Date of casting Date of Testing Specimen in e Load in Strenght Remarks
No. Mark Specimen in mm Area in sqmm Strenght Strenght h
mix Days kN inN/sqmm
inN/sqmm in N/sqmm
1 2 3 4 5 6 7 8 10 11 12 13 14
2 A-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 352 15.64 15.97 17.00 q
18.00 r
5 B-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 352 15.64 15.64 18.00 r
Average Reqd.
Age of Compressiv Compressive
Identification Concrete Dimension of Cross sectional Compre. Comp.
Sr.No. Date of casting Date of Testing Specimen in e Load in Strength Remarks
Mark mix Specimen in mm Area in sqmm Strenght Strength in
Days kN inN/sqmm
inN/sqmm N/sqmm
1 2 3 4 5 6 7 8 10 11 12 13 14
2 M-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 352 15.64 15.97 19.00 s
5 N-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 352 15.64 15.64 20.00 t
Average Reqd.
Grade of Age of Compressiv Compressive
Sr. Identification Dimension of Cross sectional Compre. Comp.
Concrete Date of casting Date of Testing Specimen in e Load in Strenght Remarks
No. Mark Specimen in mm Area in sqmm Strenght Strenght h
mix Days kN inN/sqmm
inN/sqmm in N/sqmm
1 2 3 4 5 6 7 8 10 11 12 13 14
2 P-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 352 15.64 15.97 21.00 u
21.00 u
5 R-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 352 15.64 15.64 22.00 v
Average Reqd.
Age of Compressiv Compressive
Identification Concrete Dimension of Cross sectional Compre. Comp.
Sr.No. Date of casting Date of Testing Specimen in e Load in Strength Remarks
Mark mix Specimen in mm Area in sqmm Strenght Strength in
Days kN inN/sqmm
inN/sqmm N/sqmm
1 2 3 4 5 6 7 8 10 11 12 13 14
23.00 w
2 J-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 352 15.64 15.97 23.00 w
5 K-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 352 15.64 15.64 24.00 x
Average Reqd.
Grade of Age of Compressiv Compressive
Sr. Identification Dimension of Cross sectional Compre. Comp.
Concrete Date of casting Date of Testing Specimen in e Load in Strenght Remarks
No. Mark Specimen in mm Area in sqmm Strenght Strenght h
mix Days kN inN/sqmm
inN/sqmm in N/sqmm
1 2 3 4 5 6 7 8 10 11 12 13 14
1 A-1 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 364 16.18
2 A-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 352 15.64 15.97 25.00 y
5 B-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 352 15.64 15.64 26.00 z
Average Reqd.
Age of Compressiv Compressive
Identification Concrete Dimension of Cross sectional Compre. Comp.
Sr.No. Date of casting Date of Testing Specimen in e Load in Strength Remarks
Mark mix Specimen in mm Area in sqmm Strenght Strength in
Days kN inN/sqmm
inN/sqmm N/sqmm
1 2 3 4 5 6 7 8 10 11 12 13 14
2 D-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 352 15.64 15.97 27.00 a
5 E-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 352 15.64 15.64 28.00 b
Name of Work:- S.R. to Bridge on SH-54 to Rashin Alsunde Nimbe Khatgaon Loni Masadppur
to MDR 8 Chapadgaon road, MDR.101 @ Km 1/100 tal- Karjat Dist-
Ahmednagar
Referance:- Your letter No Camp. Dated 15/03/2022.
With referance to above letter, the test results for the work cited above
are enclosed herewith for your information please.
Testing charges amounting Rs. 2920 are received on online payment receipt
Transaction No 1895306723 Dated 12/09/2022. for the same Is enclosed herewith .
Copy :- M/s Bajarangbali Construction Pp Mohan Damoder Godse At Therwadi Post Benwadi Tal. Karjat Dist Ahmednagar
VIGILANCE & QUALITY CONTROL CIRCLE NASIK
DIST. LABORATORY AHMEDNAGAR
Checklist for acceptance of sample.
1) Name and address of organization Sub Divisional Engineer P.W.Sub Division Karjat
2) Name of agency M/s Bajarangbali Construction Pp Mohan Damoder Godse At Therwadi
Post Benwadi Tal. Karjat Dist Ahmednagar
3) Details of samples.
i)Name of work S.R. to Bridge on SH-54 to Rashin Alsunde Nimbe Khatgaon Loni
Masadppur to MDR 8 Chapadgaon road, MDR.101 @ Km 1/100 tal-
Karjat Dist- Ahmednagar
ii)Material/Location.
iii)Quantity
4) Date of receipt of sample. 15/09/2022.
5) Whether samples are accompained with letter Yes
if yes,then give letter No. and date Camp. Dated 15/03/2022.
if no, samples are not accepted
6) Details of tests to be conducted and testing charges
D.S.R. Item
Sr. No. Materialas Name of tests No. of tests Rate Amount
No.
7) Whether samples are marked with lables Y/N Yes Total 2920
by the organisation
if no samples are not accepted
8) Whether the quantity of samples are Y/N Yes
adequate for testing .
9) Whether testing facility is available in the lab Y/N Yes
10) Whether serviceble and calibrated equipment Y/N Yes
are available
11) Whether trained person available for testing. Y/N Yes
11) Customer requirement if any, Y/N
13) Details of receipt of testing charges Transaction No 1895306723
Date 12/09/2022.
Rs. 2920
Recived by Approved by
R.A.
Assistant Research officer
District Laboratory Ahemadnagar.
I.S.Sieve Commulative
%age Specified limit
Sr.No. Designation Wt.Retained in gm. %age %age of passing
Retained (%age)
No. Retained
1 40 mm 0 0 0 100 100%
2 20 mm 247 2.78 2.78 97.22 85-100 %
3 10 mm 7059 79.48 82.26 17.74 0-20 %
4 4.75 mm 1427 16.07 98.32 1.68 0-5 %
5 Pan 149 1.68 100.00 0
Total 8882 100.00
SIZE OFAGGREGATE
Thickness of
Passsing Wt. of fraction consisting at Wt. of aggregate in each fraction
Sr.No. Retained on IS guage size in
through IS least 200 pieces passing through guage
Sieve mm
Sieve
1 63 MM 50 MM W1 33.9 W1
2 50 MM 40 MM W2 27 W2
3 40 MM 25 MM W3 19.5 W3
4 25 MM 20 MM W4 13.5 W4
5 20 MM 16 MM W5 10.8 W5
6 16 MM 12.5 MM W6 8.55 W6
7 12.5 MM 10 MM W7 6.75 W7
8 10 MM 6.3 MM W8 4.89 W8
TOTAL W W*
FLAKINESS INDEX (W*/W)X100 = / 15.07%
Assist.Research Officer,
Vigilance & Quality Control(P.W.D),
Dist.Laboratory,Ahmednagar
VIGILANCE & QUALITY CONTROL CIRCLE NASHIK
DIST. LABORATORY, AHMEDNAGAR
JOB NO. AHA/22-23 / 926 / PW/ANR
NAME OF DIVISION Public Work Division Ahmednagar
NAME OF SUBDIVISION P.W.Sub Division Karjat
NAME OF WORK S.R. to Bridge on SH-54 to Rashin Alsunde Nimbe Khatgaon Loni
Masadppur to MDR 8 Chapadgaon road, MDR.101 @ Km 1/100 tal-
TYPE OF SAMPLE Karjat Dist-
Cr.Metal ForAhmednagar
Concrete
DATE OF SAMPLE 15/09/2022.
DATE OF TESTING 16/09/2022 to 20/09/2022
Total 0.00 0
W1-W2 x100
3 Silt content = 5.70 5.50
W1
Average 5.60
1 2 1 2 1 2
1000 1000 1000 1000 1000 1000 1000 1000 1000 1000 1004 1000
968 969 962 963 970 972 972 968 972 969 980 975
0 95 0 0 0 0 0 90 85 85 42
120 170 120 150 150 180 190 155 160 165 296
235 230 235 255 260 190 255 305 320 255 223
255 245 280 295 265 310 265 165 150 250 161
240 130 240 205 210 180 138 140 135 120 112
105 85 85 70 85 90 112 110 110 90 91
40 45 40 25 30 50 40 35 40 35 75
995 1000 1000 1000 1000 1000 1000 1000 1000 1000 1000
1 2 1 2 1 2
1003 1002 1007 1005 1003 1000 1004 1005 1000 1002 1000 1002
982 980 981 980 979 979 981 980 975 982 978 980
1 2 1 2 1 2
1007 1005 1002 1004 1005 1010 1004 1005 1005 1010 1005 1002
982 978 977 980 977 980 970 975 977 980 977 982
1 2 1 2 1 2
1002 1005 1000 1010 1002 1003 1003 1004 1000 1000
970 980 977 980 976 978 975 976 967 966
1 2 1 2 1 2
1 2 1 2 1 2
1 2 1 2 1 2
1 2 1 2 1 2
1 2 1 2 1 2
1 2 1 2 1 2
1 2 1 2
DIST. LABORATORY, AHMEDNAGAR
JOB NO. AHA/22-23 / 926 / PW/ANR LAB./NO./ANR:- DATE:-
NAME OF DIVISION Public Work Division Ahmednagar
NAME OF SUBDIVISION P.W.Sub Division Karjat
NAME OF WORK S.R. to Bridge on SH-54 to Rashin Alsunde Nimbe Khatgaon Loni Masadppur to MDR 8 Chapadgaon road,
MDR.101 @ Km 1/100 tal- Karjat Dist- Ahmednagar
TYPE OF SAMPLE :- Cr.Sand
DATE OF RECEIPT OF SAMPLE 15/09/2022.
DATE OF TESTING 16/09/2022 to 20/09/2022
TEST RESULT OF SAND
Specified Limits
Sr. No. Type of test Results obtained
Concrete Work Road Work
1 Silt & Clay Content (%) 5.60 Not more than 4% Not more than 10%
Total 11470
CEMNT TEST
Job No. AHA/22-23 / 926 / PW/ANR
Name of Division Public Work Division Ahmednagar
Name of Sub-Division P.W.SubDivision Jamkhed
Name of Work S.R. to Bridge on SH-54 to Rashin Alsunde Nimbe Khatgaon Loni Masadppur to MDR 8
Chapadgaon road, MDR.101 @ Km 1/100 tal- Karjat Dist- Ahmednagar
Date of Testing 16/09/2022 to 20/09/2022
Details of Sample Ultratech - 53- Grade
TEST DATA SHEET : DCCT-01
Consistency
Wt. of cement Vol. of water Percentage of
Trial Reading on Vicat app. In
taken for test in added to dry water added Consistancy Remark
No. (mm)
gm cement in cc in dry cement
2 400 120 30.00 8 Hence Consistancy is
3 400 122 30.50 5
29.75
4 400 119 29.75 6
× 400/
0.85× 29.8 25.29 1:39 5:42 30 600
100
1 400 gms 10:00 11:39 15:42
=
25.29 = 101.15 99 342 Minimum Maximum
Min Min
TEST DATA SHEET : DCCT-03
Fineness by Sieving
Wt. of cement on 90
Wt. of cement Residue in
Sr. Time of Sieving mic. Sieve retained
Trial No. before sieving % observed Average % Residue Specified Remarks
No. in Min. after sieving in gm.
in gm(W1) = 5/3×100
(W2)
1 2 3 4 5 6 7 8
1 1 100 gms 15 minutes 3.00 5.00
5% Max for PPC
2 2 100 gms 15 minutes 4.00 5.00 5.33
10% Max for OPC
3 3 100 gms 15 minutes 5.00 6.00
Reference : Consistency- Methods of Physical tests for hydraulic cement.As per I.S 4031-1997 CL.6
Setting Time- As per I.S 4031-1998 CL.7
Fineness-As per I.S 4031-1996 CL.8
Say 46 CC Average 3
Equipment used : Vicat Apparatus, Lechatelier Apparatus, CTM Vigilance & Quality Control(P.W.D),
Dist.Laboratory,Ahmednagar
VIGILANCE & QUALITY CONTROL CIRCLE NASHIK
DIST. LABORATORY, AHMEDNAGAR
Total 10120
SIZE OFAGGREGATE
Thickness of Wt. of aggregate in each
Passsing Wt. of fraction consisting at least
Sr.No. Retained on IS 200 pieces guage size in fraction passing through
through IS mm guage
Sieve
Sieve
1 63 mm 50 mm W1 0 33.9 W1 0
2 50 mm 40 mm W2 12652 27 W2 999
4 25 mm 20 mm W4 0 13.5 W4 0
5 20 mm 16 mm W5 0 10.8 W5 0
6 16 mm 12.5 mm W6 0 8.55 W6 0
8 10 mm 6.3mm W8 0 4.89 W8 0
REFERANCE :-IS 2386 PART I, MOST 2000, IS 383, PWD STD. SPECIFICATION
TESTED BY S.G. Kokate (L.A.) Assist.Reaserch Officer,
CHECKED BY Y.R. Chaudhari (R.A.) Vigilance
& Quality Control(P.W.),
Dist.Laboratory,Ahmednagar
METAL-1
40 MM METAL
Sr.No. Particular
Trial-1 Trial-2
Weight of saturated aggregate suspended in water with basket
1 (W1) 2210 2141
in water in gm.
5 Weight of of water equal to the volume of aggregate in gm. W5=W4-W3 790 764
Determined
Specified
Sample 1
60 MM 100 100%
Assist.Reaserch Officer,
TESTED BY S.G. Kokate (L.A.)
CHECKED BY Y.R. Chaudhari (R.A.) Vigilance & Quality Control(P.W.),
Dist.Laboratory,Ahmednagar
DIST. LABORATORY, AHMEDNAGAR
JOB NO. AHA/22-23 / 926 / PW/ANR LAB./NO./ANR:- DATE:-
NAME OF SUBDIVISION Sub Divisional Engineer Parner
S.R. to Bridge on SH-54 to Rashin Alsunde Nimbe Khatgaon Loni Masadppur to MDR 8 Chapadgaon road, MDR.101 @ Km
NAME OF WORK 1/100 tal- Karjat Dist- Ahmednagar
TYPE OF SAMPLE 40 MM WBM Metal
DATE OF SAMPLE 15/09/2022.
DATE OF TESTING 16/09/2022 to 20/09/2022
TEST RESULTS OF COARSE AGGREGATES
Mechanical Properties- Concrete Aggregates
1 2 3 4 5 6 7 8 9
Impact Value (Not more than) 30% 45% 40% - 30%
1 14.41
Light &Heavy
Crushing Value (Not more than) 30% 45% - 12% 23% & 17%
2 15.42 Traffic
% Water Absorption Apparent Compressive Strength (N/sqmm) Impact Value(%) Crushing Value(%)
Sourse &
Sr.No. Specific
Other Details
Gravity
Deter
Specified Determined Specified Determined Specified Specified Determined
mined
Vide Std.
Specification
Gray Blakish
1 Clause A 4.07 2.85 Vide IS 1597 Part-1 1967 40.00N/mm2 42.50 Max.30% -------- Max.30%
Rubble. 8.1Not more
than 5%
Remarks
VIGILANCE & QUALITY CONTROL CIRCLE NASHIK
DIST. LABORATORY, AHMEDNAGAR
JOB NO. AHA/22-23 / 926 / PW/ANR
NAME OF DIVISION Public Work Division , Ahmednagar
NAME OF SUBDIVISION P.W.SubDivision Karjat
NAME OF WORK S.R. to Bridge on SH-54 to Rashin Alsunde Nimbe Khatgaon Loni
Masadppur to MDR 8 Chapadgaon road, MDR.101 @ Km 1/100 tal-
TYPE OF SAMPLE :-Rubble
Karjat Dist- Ahmednagar
DATE OF SAMPLE 1/28/2019
DATE OF TESTING 28/01/2019 to 31/01/2019
1 Fineness (%) 5.00 ……. ……. 10% for OPC 5% for PPC
2 Setting Time(Min)
Initial 70 min ……. ……. Not less than 30 minutes.
Final 420 min ……. ……. Not More than 600 minutes.
3 Compresive Strength in N/sqmm Curing Period 33 Grade 43 Grade 53Grade
For 3Days 28.00 ……. ……. For 3 Days 16 N/mm² 23 N/mm² 27 N/mm²
For 7Days 38.13 ……. ……. For 7 Days 22 N/mm² 33 N/mm² 37 N/mm²
For 28Days ……. ……. For 28 Days 33 N/mm² 43 N/mm² 53 N/mm²
Soundness by Le-Chateliar
4 5 ……. ……. Expansion not more than 10 mm
Apparatus mm
5 Specific Gravity 3.14 ……. ……. 3.10 to 3.15
6 Std. Consistancy 30.8 ……. ……. Not Specified
Tral Wt. of cement taken for test in Vol. of water added to Percentage of water
Reading on Vicat app. In (mm) Consistancy Remark
No. gm dry cement in cc added in dry cement
1 400 119 29.8 11 Hence Consistancy is
2 400 124 31.0 4 30.75
3 400 123 30.8 6
1 2 3 4 5 6 7 8 9
Reference : Consistency- Methods of Physical tests for hydraulic cement.As per I.S 4031-1997 CL.6
Setting Time- As per I.S 4031-1998 CL.7
Tested by : S.G. Kokate (L.A.)
Checked by : Y.R. Chaudhari (R.A.) Assist.Reaserch Officer,
Vigilance
Equipment used : Vicat apparatus and Vicat mould. & Quality Control(P.W.),
Dist.Laboratory,Ahmednagar
VIGILANCE & QUALITY CONTROL CIRCLE NASHIK
DIST. LABORATORY, AHMEDNAGAR
TEST DATA SHEET : DCCT-03
Cement Tests
JOB NO. AHA/22-23 / 926 / PW/ANR
NAME OF DIVISION Public Work Division , Ahmednagar
NAME OF SUBDIVISION P.W.Sub Division Karjat
NAME OF WORK S.R. to Bridge on SH-54 to Rashin Alsunde Nimbe Khatgaon Loni Masadppur to MDR 8 Chapadgaon road, MDR.101 @ Km 1/100 tal- Karjat Dist- Ahmed
Soundness of cement
Sr. No. Wt. of cement taken for test in Requirement of water V Actual water requirement in CC Distance separating the indicater point in
gm =0.78 x P = (V X 200) mm Limits as per IS Ref.
P=Std. consistancy 100 Initial Final Diff.
22 27 5
0.78× 30.75 23.985 × 200 26 32 6 Expansion Not More Than
1 200 gms
= 23.985 = 47.97 23 27 4 10 mm
Say 48 CC Average 5
1 2 3 4 5 6 7 8 9 10 11 12
1 30.75 200 gms 600 gms 85.5 2/18/2019 2/21/2019 3 142 28.40
2 30.75 200 gms 600 gms 85.5 2/18/2019 2/21/2019 3 140 28.00 28.00 27
3 30.75 200 gms 600 gms 85.5 2/18/2019 2/21/2019 3 138 27.60
4 30.75 200 gms 600 gms 85.5 2/18/2019 2/25/2019 7 190 38.00
5 30.75 200 gms 600 gms 85.5 2/18/2019 2/25/2019 7 190 38.00 38.13 37
6 30.75 200 gms 600 gms 85.5 2/18/2019 2/25/2019 7 192 38.40
1 2 3 4 5 6 7 8 9 10 11 12 13 14
Remark
15
er,
y Control(P.W.),
Ahemadnagar .
VIGILANCE & QUALITY CONTROL CIRCLE NASIK
DIST. LABORATORY, AHMEDNAGAR
× 400/
0.85× 30.3 25.71 1:10 7:00 30
100
1 400 gms 10:30 11:40 17:30
=
25.71 = 102.85 70 min 400 min Minimum
Wt. of cement on 90
Wt. of cement Residue in
Sr. Time of Sieving mic. Sieve retained
Trial No. before sieving % observed Average % Residue Specified
No. in Min. after sieving in gm.
in gm(W1) = 5/3×100
(W2)
1 2 3 4 5 6 7 8
1 1 100 gms 15 minutes 5.00 5.00
5% Max for PPC
2 2 100 gms 15 minutes 4.00 4.00 4.67
10% Max for OPC
3 3 100 gms 15 minutes 5.00 5.00
Reference : Consistency- Methods of Physical tests for hydraulic cement.As per I.S 4031-1997 CL.6
Setting Time- As per I.S 4031-1998 CL.7
Fineness-As per I.S 4031-1996 CL.8
PAGE 1 OF 1
adppur to MDR 8
Remark
600
Maximum
Remarks
aserch Officer,
uality Control(P.W.),
tory,Ahmednagar
K
Limit
3.10 to 3.15
Requireme
nt as per
IS in
N/mm²
12
16
22
aserch Officer,
uality Control(P.W.),
tory,Ahmednagar
DIST. LABORATORY, AHMEDNAGAR
JOB NO. AHA/22-23 / 926 / PW/ANR LAB./NO./ANR.;- DATE;-
NAME OF DIVISION Public Work Divi. Ahmednagar
NAME OF SUBDIVISION P.W.SubDivision Parner
NAME OF WORK S.R. to Bridge on SH-54 to Rashin Alsunde Nimbe Khatgaon Loni Masadppur to MDR 8
Chapadgaon road, MDR.101 @ Km 1/100 tal- Karjat Dist- Ahmednagar
Equipment used : Vicat Apparatus, Lechatelier Apparatus, CTM Vigilance & Quality Control(P.W.),
Dist.Laboratory,Ahmednagar
VIGILANCE & QUALITY CONTROL CIRCLE NASHIK
DIST. LABORATORY, AHMEDNAGAR
TEST DATA SHEET : DCC-21
CONCRETE CUBE TEST
1 2 3 4 5 6 7 8 9 10 11 12 13 14
2 1:04:08 M-7.5 2/17/2018 4/13/2018 55 150x150x150 22500 8.442 210 9.33 8.89 8.02
5 1:03:06 M-10 2/19/2018 4/13/2018 53 150x150x150 22500 8.458 250 11.11 11.11 10.65
2 A-2 M-10 2/10/2018 3/12/2018 30 150x150x150 22500 8.459 240 10.67 10.81 10.01
1 2 3 4 5 6 7 8 9 10 11 12 13 14
2 D-2 M-20 7/15/2017 10/11/2017 88 150x150x150 22500 8.452 530 23.56 19.85 23.10
5 E-2 M-20 7/15/2017 10/11/2017 88 150x150x150 22500 8.454 540 24.00 24.30 23.10
2 F-2 M-20 7/15/2017 10/12/2017 89 150x150x150 22500 8.457 530 23.56 24.00 23.15
5 G-2 M-20 7/15/2017 10/12/2017 89 150x150x150 22500 8.459 540 24.00 24.30 23.15
1 2 3 4 5 6 7 8 9 10 11 12 13 14
2 H-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 8475 790 35.11 32.15 30.00 i
5 I-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 8546 750 33.33 31.85 30.00 j
2 J-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 8475 690 30.67 32.59 30.00 k
5 K-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 8546 710 31.56 32.30 30.00 l
1 2 3 4 5 6 7 8 9 10 11 12 13 14
2 M-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 8475 225 10.00 10.00 10.00 m
5 N-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 8546 225 10.00 10.00 20.00 n
2 P-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 8475 352 15.64 15.97 15.00 o
5 R-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 8546 352 15.64 15.64 16.00 p
1 2 3 4 5 6 7 8 9 10 11 12 13 14
2 A-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 8475 352 15.64 15.97 17.00 q
5 B-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 8546 352 15.64 15.64 18.00 r
2 M-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 8475 352 15.64 15.97 19.00 s
5 N-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 8546 352 15.64 15.64 20.00 t
1 2 3 4 5 6 7 8 9 10 11 12 13 14
2 P-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 8475 352 15.64 15.97 21.00 u
5 R-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 8546 352 15.64 15.64 22.00 v
2 J-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 8475 352 15.64 15.97 23.00 w
5 K-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 8546 352 15.64 15.64 24.00 x
1 2 3 4 5 6 7 8 9 10 11 12 13 14
2 A-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 8475 352 15.64 15.97 25.00 y
5 B-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 8546 352 15.64 15.64 26.00 z
2 D-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 8475 352 15.64 15.97 23.10
5 E-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 8546 352 15.64 15.64 23.10
1 2 3 4 5 6 7 8 10 11 12 13 14
2 1:04:08 M-7.5 2/17/2018 4/13/2018 55 150x150x150 22500 210 9.33 8.89 8.02
5 1:03:06 M-10 2/19/2018 4/13/2018 53 150x150x150 22500 250 11.11 11.11 10.65
2 A-2 M-10 2/10/2018 3/12/2018 30 150x150x150 22500 240 10.67 10.81 10.01
1 2 3 4 5 6 7 8 10 11 12 13 14
2 D-2 M-20 7/15/2017 10/11/2017 88 150x150x150 22500 530 23.56 19.85 23.10
5 E-2 M-20 7/15/2017 10/11/2017 88 150x150x150 22500 540 24.00 24.30 23.10
2 F-2 M-20 7/15/2017 10/12/2017 89 150x150x150 22500 530 23.56 24.00 23.15
5 G-2 M-20 7/15/2017 10/12/2017 89 150x150x150 22500 540 24.00 24.30 23.15
1 2 3 4 5 6 7 8 10 11 12 13 14
2 H-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 790 35.11 32.15 30.00 i
5 I-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 750 33.33 31.85 30.00 j
2 J-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 690 30.67 32.59 30.00 k
5 K-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 710 31.56 32.30 30.00 l
1 2 3 4 5 6 7 8 10 11 12 13 14
2 M-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 225 10.00 10.00 10.00 m
5 N-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 225 10.00 10.00 20.00 n
2 P-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 352 15.64 15.97 15.00 o
15.00 o
5 R-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 352 15.64 15.64 16.00 p
2 A-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 352 15.64 15.97 17.00 q
5 B-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 352 15.64 15.64 18.00 r
2 M-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 352 15.64 15.97 19.00 s
5 N-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 352 15.64 15.64 20.00 t
1 2 3 4 5 6 7 8 10 11 12 13 14
2 P-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 352 15.64 15.97 21.00 u
5 R-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 352 15.64 15.64 22.00 v
2 J-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 352 15.64 15.97 23.00 w
5 K-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 352 15.64 15.64 24.00 x
1 2 3 4 5 6 7 8 10 11 12 13 14
2 A-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 352 15.64 15.97 25.00 y
5 B-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 352 15.64 15.64 26.00 z
2 D-2 M-15 7/2/2013 7/30/2013 28 150x150x150 22500 352 15.64 15.97 23.10 0
5 E-2 M-15 6/25/2013 7/26/2013 31 150x150x150 22500 352 15.64 15.64 23.10 0
% Water Absorption Apparent Compressive Strength (N/sqmm) Impact Value(%) Crushing Value(%)
Sourse &
Sr.No. Specific
Other Details
Gravity
Deter
Specified Determined Specified Determined Specified Specified Determined
mined
Vide Std.
Specification
Gray Blakish
1 Clause A 4.41 2.87 Vide IS 1597 Part-1 1967 40.00N/mm2 42.50 Max.30% -------- Max.30%
Rubble. 8.1Not more
than 5%
Remarks
VIGILANCE & QUALITY CONTROL CIRCLE NASHIK
DIST. LABORATORY, AHMEDNAGAR
JOB NO. AHA/22-23 / 926 / PW/ANR
NAME OF DIVISION Public Work Division , Ahmednagar
NAME OF SUBDIVISION P.W.SubDivision Parner
NAME OF WORK S.R. to Bridge on SH-54 to Rashin Alsunde Nimbe Khatgaon Loni
Masadppur to MDR 8 Chapadgaon road, MDR.101 @ Km 1/100 tal-
TYPE OF SAMPLE :-Rubble
Karjat Dist- Ahmednagar
DATE OF SAMPLE 9/29/2018
DATE OF TESTING 29/09/2018 to 01/10/2018
Remark
15
Control(P.W.),
hemadnagar .