CONCRETE MIX DESIGN

QUALITY CONTROL LABORATORY


ACI 211.1-91

Date : 9/14/2020 Standard : ASTM


Customer Name : Beta Tech Specimen : Cylinder
Project : STC-NEIDC-P2-4DC Makkah strength @ 28d : 40 Mpa
‫ مركز بيانات لشركة‬STC Slump at site : 150±30 mm
Location : Makkah N Max Size CA : 19 mm
Temperature : 32 ˚c
Batch wt /m³

Materiale unit Type Quantity Source Sp . Gr Reference


Cement Kg SRC 440 Yanbu 3.15 ASTM C150
Microsilica Kg m.s 0 Masheed 2.2 ASTM C1240
3/4" Aggregates Kg Crushed 548 saud alsaadi 2.85 ASTM C33
1/2" Aggregates Kg Crushed 0 saud alsaadi 2.84 ASTM C33
3/8" Aggregates Kg Crushed 448 saud alsaadi 2.82 ASTM C33
Sand Kg natural 828 Makkah 2.63 ASTM C33
free water Kg 168 Tahlia 1 ASTM C94
Admixture 1 Kg Sp 8.5 Weber 1.218 ASTM C494
Admixture 2 Kg Ret. 0.0 Weber 1.100 ASTM C494
Air Voids 2.0% ASTM C231
Total 2441
volume/m³ proportion of aggregates Water
cement 0.1397 0.9 45.4% Free water 168
Micro silica 0.0000 C. Agg 54.6% Adjustment 18
Water 0.1680 3/4 C.Agg 55% Total water 186
Volume of Air Voids 0.0200
Volume of 3/4" 0.1923 3/8 C.Agg 45%
Volume of 1/2" 0.0000
Volume of 3/8" 0.1589
Volume of sand 0.3148
Volume of Add1 0.0070
Volume of Add2 0.0000
Total Volume 1.00 F.M 2.7 W/C 0.38
Remarks
*to increase workability at site type F plasticizer can be add 1 liter /m3
*During the trial mix we can use the actual absorption and moisture
*During the trial mix we can increase or reduce admixture depending on nature of material

Note prepared by
Use concrete before 120 minutes from the time of batching Eng / Shamshad Ali