TENSILE TEST CERTIFICATE

REPORT NO. :- D24 Sample Description :-CS Product Test Coupon


TEST DATE :- 15-11-23 Material Specification :- ASME SA234 WPB-Edn.2019 SEC-II, PT-A
TEST EQUIPMENT :- FIEL-UTM-200 KN Test Method :- ASTM A370
STAMPED BY :- Sr No. :-8/2019-6307 LAST CALIBRATION DATE: 06-02-2024

TEST RECORD
SR. NO. 1 Required Values Min.

PIPE SIZE 100NB S40


DN100 X DN80 S40 BW UNEQ TEE, DN100 X DN50 S40 BW UNEQ TEE, N100 X DN50
FITTING S40 BW ER RED, DN100 X DN80 S40 BW CR RED, DN100 X DN50 S40 BW CR RED,
MANUFACTURED DN100 S40 BW END CAP, DN100 S40 EQ TEE
HEAT NO. AA2167
Sample Direction Longitudinal
Thickness mm 6.02
Breadth mm 19.05
Area mm² 114.7
Gauge Length mm 50
Final lengt mm 64.3
Final dia mm -
Yield Load KN 35.2
Ultimate Load KN 49.3
Y. S. N/mm²(0.2% Offset) 306.9 Min 240
U.T.S N/mm² 429.9 Min 415–585
% Reduction Area mm² -
% Elongnation 28.6 22%

Fracture WGL
Hadrness Test Method ASTM E 10 :2017
Location Surface
Hardness 10 mm dia Ball /29.42 KN/3000 kgf
Ball dia 5 MM
Hardness(HRB) -
Hardness(BHN) 142.6 197 BHN MAX
Bend Test OK
Remark Satisfactory

Tested By Witnessed By